Silver nano cubic auxiliary agent, preparation method, dispersion method and application
The chemical reduction reaction of silver nitrate and ascorbic acid is combined with the stabilizer of polyvinylpyrrolidone to control the reaction conditions to prepare silver nanocubes, and improve its dispersion through physical dispersion technology, which solves the problems of complex preparation process and poor stability of silver nanocubes. , achieving efficient and stable silver nanocube additives, improving their performance in a variety of applications.
Patent Information
- Application Number
- CN202410806490.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-29
AI Technical Summary
The preparation process of silver nanocubes is complex, the particle size distribution is uneven, and the stability is poor, which limits its further promotion in practical applications.
Silver nitrate and ascorbic acid are used as metallic silver precursors and reducing agents, combined with polyvinylpyrrolidone as a stabilizer. By controlling reaction conditions such as temperature, pH value and reaction time, a chemical reduction reaction is performed to prepare silver nanocubes, and through physical dispersion technology Such as ultrasonic treatment and chemical dispersants to improve its dispersion.
It achieves efficient, stable preparation and uniform dispersion of silver nanocubes, improves its application performance in fields such as catalysis, electromagnetic shielding and conductive coatings, and has the advantages of environmental protection, safety and cost-effectiveness.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electronic packaging materials and thermal conductive interface material additives, and in particular to a silver nanocube additive, a preparation method, a dispersion method and an application thereof. Background Art
[0002] With the rapid development of nanotechnology, nanomaterials have shown broad application prospects in various fields due to their unique physical and chemical properties. In particular, silver nanomaterials have become a hot material in scientific research and industrial production due to their good antibacterial, electrical and thermal conductivity. Among them, silver nanocubes, as a nanomaterial with regular morphology, have shown great application potential in catalysts, sensors, biomedicine and other fields due to their unique surface effects and size effects.
[0003] However, there are still some challenges in the preparation and dispersion technology of silver nanocubes, such as complex preparation process, uneven particle size distribution, poor stability and other problems, which limit its further promotion in practical applications. Specifically, the current preparation methods of silver nanocubes mainly include physical methods, chemical methods and biological methods. Among them, the chemical method has become the most commonly used preparation method due to its advantages such as simple operation and low cost. However, traditional chemical preparation methods often have problems such as complex preparation process, harsh reaction conditions, and uneven product particle size distribution. In addition, silver nanocubes are prone to agglomeration during the preparation process, resulting in a decrease in their performance in applications. Therefore, the development of a simple, efficient and controllable method for preparing and dispersing silver nanocubes has important research significance and application value. Summary of the invention
[0004] The main purpose of the present invention is to provide a silver nanocube auxiliary agent, a preparation method, a dispersion method and an application, aiming to improve the technical problems of the existing silver nanocubes, such as complex preparation process, uneven particle size distribution and poor stability.
[0005] To achieve the above object, the present invention provides a method for preparing a silver nanocube additive, comprising the following steps:
[0006] 1) mixing a metallic silver precursor and a reducing agent in a solution to obtain a mixed solution, and adjusting the pH value of the mixed solution to 6-8;
[0007] 2) heating the mixed solution obtained in step 1) to 40-60° C. for reaction for 2-4 hours;
[0008] 3) After the reaction in step 2) is completed, the silver nanocubes are separated by centrifugation and washing, and then dried to obtain the silver nanocube auxiliary agent.
[0009] Preferably, in step 1), the metallic silver precursor is silver nitrate, and the reducing agent is ascorbic acid.
[0010] Preferably, in step 1), the solution includes a stabilizer, which is polyvinyl pyrrolidone, and further includes deionized water, wherein the concentration of the stabilizer is sufficient to ensure the stability and dispersibility of the silver nanocubes during the preparation process.
[0011] In this scheme, a suitable metallic silver precursor and a reducing agent are selected, wherein the metallic silver precursor is silver nitrate and the reducing agent is ascorbic acid; the metallic silver precursor and the reducing agent are mixed in a solution, wherein the solution contains a stabilizer, and the stabilizer is polyvinyl pyrrolidone (PVP); the pH value of the solution is adjusted to a predetermined range, specifically between 6 and 8; the mixed solution is heated to 40-60° C. and maintained for 2-4 hours; after the reaction is completed, the silver nanocubes are separated by centrifugation and washing steps, and dried to obtain the final product.
[0012] Preferably, in step 3), the drying process is carried out under vacuum conditions. The drying process is carried out under vacuum conditions to prevent oxidation of the silver nanocubes.
[0013] In addition, the present invention also provides a silver nanocube auxiliary agent, which is prepared by any of the above-mentioned methods for preparing the silver nanocube auxiliary agent.
[0014] In addition, the present invention also provides a method for dispersing a silver nanocube auxiliary agent, comprising the following steps: mixing the silver nanocube auxiliary agent with a dispersion medium and then physically dispersing the mixture to obtain a dispersed silver nanocube auxiliary agent.
[0015] Preferably, a dispersant is added to the physically dispersed silver nanocube auxiliary agent, and the dispersant is a nonionic surfactant, a cationic surfactant or an anionic surfactant.
[0016] Preferably, the dispersion medium is an aqueous solvent or an organic solvent.
[0017] Preferably, the physical dispersion method comprises ultrasonic treatment or mechanical stirring. The amount of physical dispersion technology and chemical dispersant used can be adjusted according to the specific requirements of the desired application.
[0018] The silver nanocubes prepared as described above are mixed with a dispersion medium; a physical dispersion technique is used to disperse the silver nanocubes, such as ultrasonic treatment or mechanical stirring treatment, to improve the dispersibility of the silver nanocubes in the dispersion medium; a chemical dispersant may also be added to the dispersion medium to further improve the dispersibility; finally, the dispersed silver nanocubes are applied to a target medium or substrate.
[0019] In addition, the present invention also proposes an application of the silver nanocube additive, which is applied in the fields of catalysis, electromagnetic shielding or conductive coating.
[0020] The silver nanocubic block additive applicable here is obtained by the preparation method of the silver nanocubic block additive mentioned above, and can be dispersed by the dispersion method of the silver nanocubic block additive mentioned above. The silver nanocubic block additive is applied in catalysis, electromagnetic shielding or conductive coating or any other field requiring the characteristics of silver nanoparticles. The silver nanocubic block additive has the characteristics of increasing reaction rate, enhancing electromagnetic shielding effect or improving electrical conductivity. In addition, the size and shape of the (dispersed) silver nanocubic block additive prepared in this scheme make it particularly suitable for the above-mentioned specific application requirements.
[0021] Compared with the prior art, the present invention provides a silver nanocube additive, a preparation method, a dispersion method and an application, which have the following beneficial effects:
[0022] 1. The present invention provides an efficient and stable silver nanocube preparation technology, and ensures the uniform dispersion of the prepared silver nanocube in application. First, in the preparation method, silver nanoparticles with a cubic shape are synthesized under controlled conditions through a specific chemical reduction reaction. The preparation process includes selecting suitable metal precursors, reducing agents and stabilizers, and accurately controlling reaction conditions such as temperature, pH value and reaction time to obtain silver nanocubes with uniform size and regular shape. The dispersion method of the present invention improves the dispersibility of silver nanocubes in the medium through physical and chemical means, thereby improving its performance in various applications, so that the silver nanocube additive of the present invention shows excellent application potential in the fields of catalysis, electromagnetic shielding, conductive coatings, etc.
[0023] 2. Environmental protection and safety: The present invention adopts environmentally friendly materials and reaction systems when preparing or dispersing silver nanocube additives, thereby reducing potential risks to the environment and human health.
[0024] 3. Cost-effectiveness: Compared with many existing metal nanoparticle synthesis methods, the preparation method of the present invention has lower costs because cost-effective starting materials are used, and the entire preparation process is simple, efficient, and suitable for large-scale production.
[0025] 4. Chemical stability: The silver nanocube additives prepared by the above preparation method have excellent chemical stability, which means that they can maintain stable performance under a wide range of conditions and can achieve long-term application and long-term storage. DETAILED DESCRIPTION
[0026] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the fact that ordinary technicians in the field can implement it. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0028] The present invention aims to provide a simple, efficient and reliable preparation method and dispersion method for producing silver nanocubes with uniform size and regular shape, and ensuring that these silver nanocubes (particles) can maintain good dispersibility in applications.
[0029] Preparation method of silver nanocube additive:
[0030] (1) Raw material selection: The raw materials used in this method include silver nitrate (AgNO3) as a silver precursor, ascorbic acid as a reducing agent, and polyvinyl pyrrolidone (PVP) as a stabilizer.
[0031] (2) Synthesis steps: First, silver nitrate and ascorbic acid are dissolved in deionized water in proportion, and then the pre-dissolved PVP solution is added. After mixing evenly, the solution is heated to 40-60°C and kept at a constant temperature for 2-4 hours. During the entire reaction process, PVP acts as a stabilizer to prevent silver nanoparticles from aggregating and controls their growth rate to ensure the formation of a cubic shape.
[0032] (3) Post-treatment: After the reaction is completed, unreacted chemicals and by-products are removed by centrifugation and multiple washings to obtain pure silver nanocube powder. The powder can be dried in a vacuum drying oven for subsequent use.
[0033] Dispersion method of silver nanocube additive:
[0034] (1) Physical dispersion: Physical dispersion of silver nanocubes is performed using ultrasonic treatment / mechanical stirring methods. Silver nanocube powder is added to a suitable solvent (such as ethanol or water) and then treated with an ultrasonic oscillator to break up the agglomeration between particles.
[0035] (2) Chemical dispersion: The dispersibility of the silver nanocubes can be further improved by adding an appropriate amount of surfactant (such as sodium dodecyl sulfate SDS). The surfactant can reduce the surface energy of the silver nanocubes, thereby reducing the possibility of particle reaggregation.
[0036] In order to solve the problems existing in the traditional silver nanocube preparation and dispersion methods, the present invention proposes the above-mentioned new preparation and dispersion method of the silver nanocube auxiliary agent. The method adopts rapid synthesis technology, silver nitrate provides the silver source, ascorbic acid is used as a reducing agent, polyvinyl pyrrolidone (PVP) is used as a stabilizer, sodium dodecyl sulfate and the like are used as surfactants, and the efficient preparation of the silver nanocube is achieved by optimizing the reaction conditions and controlling the reaction process, and the uniform dispersion of the silver nanocube is achieved by the subsequent dispersion method. The above-mentioned preparation method has the advantages of easy availability of raw materials, simple process, easy acquisition of equipment, easy operation of the process, short production time, high efficiency and uniform size of the product nano silver cube.
[0037] The invention not only provides a new idea and method for the preparation of silver nanocubes, but also provides strong support for the application of silver nanocubes in the fields of catalysts, sensors, biomedicine, etc. Through the above preparation and dispersion method, a silver nanocube additive with regular morphology, uniform particle size and good stability can be prepared, thereby improving its performance and effect in application.
[0038] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention, and are not used to limit the present invention.
[0039] In the preparation process of the following examples, the reaction system should be kept in a vacuum-tight state to avoid volatilization and oxidation of ethylene glycol. The stirring speed and stirring time have an important influence on the formation and particle size distribution of silver nanocubes and need to be optimized according to specific experimental conditions. During the washing and drying process, the solid matter should be ensured to be fully cleaned and thoroughly dried to avoid residual impurities and agglomeration.
[0040] Example 1
[0041] 1. Experimental Materials
[0042] Raw materials: silver nitrate (AgNO3), polyvinyl pyrrolidone (PVP), ethylene glycol (EG), ascorbic acid.
[0043] Solvent: Ethylene glycol solution.
[0044] 2. Experimental steps for preparing silver nanocube additives
[0045] 1) preparing a solution: mixing a polyvinyl pyrrolidone glycol solution having a concentration of 0.5 mol / l (a concentration range of 0.3-0.75 mol / l), a silver nitrate glycol solution having a concentration of 0.4 mol / l (a concentration range of 0.2-0.5 mol / l) and an ascorbic acid glycol solution having a concentration of 0.18 mol / l (a concentration range of 0.034-0.27 mol / l) in a volume ratio of 1:0.4:0.2 (a volume ratio range of 1:0.3-1:0.1-0.4) to obtain a mixed solution, and adjusting the pH value of the mixed solution to 7;
[0046] 2) Stirring: Stir the mixed solution for at least 1 min (stirring time range is 1-3 min) at a stirring speed of 1000 r / min;
[0047] 3) Reaction: In a sealed state, the mixed solution is reacted at 45° C. for 2 h to obtain a reaction solution;
[0048] 4) Cooling and solid-liquid separation: After the reaction liquid is cooled to room temperature, solid-liquid separation is performed, specifically, centrifugation is performed for 8 minutes (the centrifugation time range is 5-10 minutes) at a speed of 8000 r / min (the speed range is 7000-9000 r / min);
[0049] 5) Washing: The separated solids are washed 4 times with deionized water, and the solids are separated by centrifugation during washing;
[0050] 6) Drying: The cleaned solid matter is dried at 65° C. (drying temperature is 40-70° C.) to obtain silver nanocubes with a side length of 40-150 nm.
[0051] Example 2
[0052] A method for preparing a silver nanocube additive comprises the following steps:
[0053] 1) preparing a solution: mixing a 0.6 mol / l polyvinyl pyrrolidone ethylene glycol solution, a 0.35 mol / l silver nitrate ethylene glycol solution and a 0.06 mol / l ascorbic acid ethylene glycol solution in a volume ratio of 1:0.6:0.1 to obtain a mixed solution, and adjusting the pH value of the mixed solution to 6;
[0054] 2) Stirring: Stir the mixed solution for at least 1 min at a stirring speed of 1000 r / min;
[0055] 3) Reaction: In a sealed state, the mixed solution is reacted at 45° C. for 2 h to obtain a reaction solution;
[0056] 4) Cooling and solid-liquid separation: After the reaction liquid is cooled to room temperature, solid-liquid separation is performed, specifically, centrifugation is performed for 6 minutes at a speed of 8500 r / min;
[0057] 5) Washing: The separated solid matter is washed 5 times with ethanol, and the solid matter is still separated by centrifugation during washing;
[0058] 6) Drying: The cleaned solid matter is dried at 58° C. (drying temperature is 40-70° C.) to obtain silver nanocubes with a side length of 40-150 nm.
[0059] The silver nanocube additive prepared by the above method has the advantages of small particle size, uniform size, high yield, etc. At the same time, due to the high temperature and high pressure reaction conditions used in the preparation process, the obtained silver nanocube additive has excellent stability and dispersibility, which can meet the application needs of different fields.
[0060] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for preparing a silver nanocube additive, It is characterized in that The steps include: 1) mixing a metallic silver precursor and a reducing agent in a solution to obtain a mixed solution, and adjusting the pH value of the mixed solution to 6-8; 2) heating the mixed solution obtained in step 1) to 40-60° C. for reaction for 2-4 hours; 3) After the reaction in step 2) is completed, the silver nanocubes are separated by centrifugation and washing, and then dried to obtain the silver nanocube auxiliary agent.
2. A method for preparing a silver nanocube additive according to claim 1, It is characterized in that In step 1), the metallic silver precursor is silver nitrate, and the reducing agent is ascorbic acid.
3. The method for preparing a silver nanocube additive according to claim 1, It is characterized in that In step 1), the solution includes a stabilizer, and the stabilizer is polyvinyl pyrrolidone.
4. The method for preparing a silver nanocube additive according to claim 1, It is characterized in that In step 3), the vacuum condition is maintained during the drying process.
5. A silver nanocube additive, It is characterized in that The silver nanocube additive is prepared by the preparation method of the silver nanocube additive according to any one of claims 1 to 4.
6. A method for dispersing silver nanocube additives, It is characterized in that The method comprises the following steps: mixing the silver nanocube auxiliary agent described in claim 5 with a dispersion medium and then physically dispersing the mixture to obtain the dispersed silver nanocube auxiliary agent.
7. A method for dispersing a silver nanocube additive according to claim 6, It is characterized in that A dispersant is added to the physically dispersed silver nanocube auxiliary agent, wherein the dispersant is a nonionic surfactant, a cationic surfactant or an anionic surfactant.
8. The method for dispersing a silver nanocube additive according to claim 6, It is characterized in that The dispersion medium is an aqueous solvent or an organic solvent.
9. The method for dispersing a silver nanocube additive according to claim 6, It is characterized in that The physical dispersion method includes ultrasonic treatment or mechanical stirring.
10. A use of the silver nanocube additive as claimed in claim 5, It is characterized in that The silver nanocube additive is used in the fields of catalysis, electromagnetic shielding or conductive coating.