Titanium alloy friction stir welding defect control method

Through back arc preheating and back penetration forced forming groove structure, combined with the coupling of arc heat source and friction stir welding, the problem of titanium alloy welding defects is solved, and efficient, high-quality medium-thickness and high-strength titanium alloy welding is achieved, which meets the needs of aerospace and aerospace industries. Strict requirements for marine engineering.

CN118848201APending Publication Date: 2024-10-29NORTHWESTERN POLYTECHNICAL UNIV +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411166879.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

It is difficult to achieve efficient, defect-free and high-quality friction stir welding of titanium alloys with existing technology, especially in medium-thick and high-strength titanium alloy materials, which are prone to welding defects such as weak root bonding, incomplete welding and tunnel defects, and the existing heating The method is inefficient and cannot meet the strict requirements of aerospace and marine engineering.

Method used

Use back arc preheating to heat titanium alloy materials, design a welding tool with a stirring pin length greater than the thickness of the workpiece, and use a back penetration forced forming groove structure to replace the welding pad during the welding process. Through the coupling of the arc heat source and friction stir welding, the The plasticity and fluidity of the material reduce welding resistance, the spiral side grooves and grooves are designed to increase the contact area, and high-purity argon gas is used for protection.

Benefits of technology

It effectively reduces the occurrence of welding defects, improves welding efficiency and quality, reduces welding tool wear, and achieves high-strength, high-quality titanium alloy welded joints that meet the performance requirements of aerospace and marine engineering.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118848201A_ABST
    Figure CN118848201A_ABST
Patent Text Reader

Abstract

The invention discloses a titanium alloy friction stir welding defect control method, and relates to the technical field of metal material welding. The method comprises the steps that a to-be-welded workpiece is heated through an auxiliary heat source electric arc, and when the to-be-welded workpiece reaches a plastic state, a stirring needle is inserted to conduct penetration welding through a back penetration welding forced forming groove; wherein during welding, an electric arc is arranged in front, and to-be-welded front-side metal of a stirring needle is heated; according to the method, a process window is effectively widened, welding defects are reduced, welding tool abrasion is reduced, and therefore high-quality friction stir welding of the medium-thickness high-strength titanium alloy is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal material welding, and in particular to a titanium alloy friction stir welding defect control method. Background Art

[0002] The great achievements made by my country's aviation, aerospace and marine engineering in the 21st century are closely related to the development of lightweight, high-strength materials and dissimilar materials. New structural materials, such as titanium alloys, are gradually replacing conventional aluminum alloys and structural steels, and are used in aerospace engines, flap rails, ships and marine engineering. The performance and quality requirements of aerospace and marine engineering materials are extremely strict. In a variety of processing and manufacturing, welding is the key forming process of structural parts. Among them, friction stir welding (FSW) has become one of the research hotspots of lightweight structural material welding due to its good practicality, reliability and economy. The peak temperature of the FSW process is only 60%-80% of the melting point of the material, which puts higher requirements on the high-temperature mechanical properties and wear resistance of the stirring head material. For lightweight and high-strength materials, especially high-melting point materials, the material rheological stress is large during the welding process, so the joint is prone to weak connection, tunnel and other forming defects, resulting in a decrease in joint quality. Therefore, reducing the rheological resistance of titanium alloys and improving welding efficiency to achieve metallurgical bonding, thereby achieving its efficient and high-quality connection, is the frontier and difficult problem in the current research field of friction stir welding.

[0003] In response to the above problems, researchers have developed a number of technologies to solve them. CN202726313U ultrasonic vibration assisted friction stir welding device and CN102744516B ultrasonic vibration assisted friction stir welding process and device are both related technologies developed for aluminum alloy friction stir welding, and have significant effects on efficient and high-quality connection of aluminum alloys. However, its applicability to high melting point and high-strength titanium alloys is limited, and the ultrasonic solid phase plasticization effect is not suitable for titanium alloy friction stir welding. CN108907448A is a friction stir welding process method for mobile heating of the back of thick copper and aluminum dissimilar metals. The workpiece to be welded is horizontally fixed on a ceramic panel, and the steel pad is heated by the alternating magnetic field of an induction furnace. The steel pad transfers heat to the back of the weldment, but the controllability of the heating temperature and the heating efficiency are low, and it is not suitable for long-distance continuous welding. It is also not applicable to titanium alloys with poor thermal conductivity. Two patents are available: a friction stir welding process method that combines back heating and front cooling, and a method for improving the temperature gradient in the thickness direction of thick aluminum alloy friction stir welding. The back heating device used in the former is a long block heating plate structure, the heating area is integrated, and the heating temperature is not easy to adjust, resulting in the heating device being not targeted and having low thermal efficiency; the latter uses a mobile high-frequency induction coil heating device to directly heat the back of the aluminum alloy thick plate, which cannot solve the problem of process support on the back of the weld. CN103028838B electromagnetic plastic friction stir welding tool and method are used to solve the problems of residual stress, hole defects, and poor weldability in existing friction stir welding joints. This invention method is different from resistance heat-assisted friction stir welding. It strictly limits the effect of resistance heat and uses internal electrons to promote dislocation movement, thereby improving the plasticity of the material. At the same time, based on the principle of electroplasticity, a rotating magnetic field is further added. The rotating magnetic field acts on the pulse current to make the orientation of the electron force instantaneously diversified, thereby promoting dislocation sliding to the greatest extent. The improvement effect on dislocation accumulation, blockage, and entanglement is far greater than the directional electron force of the pulse current. However, since titanium alloys are non-magnetic, this method is not applicable to titanium alloys. There is no relevant report on the arc-assisted friction stir welding method. Summary of the invention

[0004] In view of the deficiencies in the above-mentioned background technology and the demand for efficient, defect-free and high-quality friction stir welding of medium-thick and high-strength titanium alloys with a thickness of more than 6 mm, the present invention provides a defect control method for friction stir welding of titanium alloys. The method effectively broadens the process window, reduces defects such as weak bonding, incomplete penetration and tunneling at the welding root, reduces welding tool wear, and thus achieves high-quality friction stir welding of medium-thick and high-strength titanium alloys.

[0005] The first object of the present invention is to provide a titanium alloy friction stir welding defect control method, comprising the following steps: The workpiece to be welded is heated by an auxiliary heat source arc, and when the workpiece reaches a plastic state, a stirring pin is inserted for penetration welding; during welding, the arc is placed in front to heat the metal to be welded in front of the stirring pin; Use positive and back gas protection to protect the molten pool and high temperature area after welding; Set the stirring needle length to be greater than the workpiece thickness; A back penetration forced forming groove is arranged at the back of the weld, the notch of the back penetration forced forming groove faces the weld and is used to accommodate the semi-solid plastic metal stirred and extruded by the end of the stirring pin; the back penetration forced forming groove corresponds to the stirring pin; During the welding process, the stirring needle and the back penetration forced forming groove are relatively stationary, and the workpiece to be welded is moved between the stirring needle and the back penetration forced forming groove.

[0006] Preferably, the inner cavity of the back penetration forced forming groove is an inverted conical cavity with a groove depth of 0.2-1mm, and is consistent with the shape of the top of the stirring needle. The front of the groove is tightly attached to the position of the weld to be welded, and the center of the groove coincides with the center line of the weld.

[0007] Preferably, a welding gun generating an auxiliary heat source arc is fixed on the friction stir welding equipment, and the spatial position of the tungsten electrode is adjusted by rotating a shrink sleeve and a telescopic rod; wherein the arc adopts a tungsten electrode having a size of 5-10 mm and a frustum design, and the top size of the frustum is 2-5 mm, so as to obtain a defocused arc.

[0008] Preferably, the surface of the stirring needle is provided with spiral side grooves with a helix angle of 6-8° and grooves along the axis direction of the stirring needle.

[0009] Preferably, the arc and the stirring needle are on the same welding axis, the arc is located at the front of the stirring needle welding path, and the distance between the two is related to the welding power. When the welding power is greater than 500 watts, the distance between the two is greater than 5 mm, otherwise the distance between the two is less than 5 mm.

[0010] Preferably, the protective gas used is argon with a purity of 99.999% and a flow rate of 10-30 L / min.

[0011] A second object of the present invention is to provide a welded titanium alloy workpiece.

[0012] The third object of the present invention is to provide a welded titanium alloy workpiece for use in aircraft engines, flap rails, aerospace, ships or marine engineering.

[0013] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides a titanium alloy stir friction welding defect control method, which improves the plasticity of the back of the titanium alloy stir welding through back arc preheating, enhances the plastic deformation capacity of the material, designs a welding tool with a stirring needle length greater than the thickness of the workpiece to achieve penetration welding, and replaces the welding pad with a back penetration forced forming groove structure to achieve axial support, and opens a semi-solid plastic metal stirred and extruded by the end of the stirring needle in the center of the back penetration forced forming groove to achieve penetration stir friction welding, thereby effectively avoiding the generation of root unfusion and weak bonding defects.

[0014] The welding method provided by the present invention designs spiral side grooves with a helix angle of 6-8° and grooves along the axis direction of the stirring needle on the surface of the stirring needle to increase the contact area between the stirring needle and the plate, improve the flow filling capacity of the plastic metal, and help to obtain a fully filled and defect-free welding joint.

[0015] The welding method provided by the present invention improves the plasticity and fluidity of the material to be welded, reduces the welding resistance in the welding process, and reduces the wear of the stirring tool through the coupling of the arc heat source and the temperature field and flow field of the stir friction welding. The arc adopts a large tungsten pole and a truncated cone design to obtain a defocused arc, so that the material to be welded can be fully heated and softened, solving the problem that welding defects are easily generated in the stir welding of titanium alloys with a thickness of more than 6 mm. By controlling the rotation speed and welding speed of the stirring head, the microstructure of the weld is controlled to achieve the purpose of controllable organization. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 Schematic diagram of the friction stir welding process with auxiliary heat source penetration.

[0017] Figure 2 Schematic diagram of the back forced forming groove and stirring pin remaining relatively still.

[0018] Figure 3 It is a stirring head for friction stir welding of medium and thick titanium alloys. DETAILED DESCRIPTION

[0019] In order to enable those skilled in the art to better understand and implement the technical solution of the present invention, the present invention is further described below in conjunction with specific embodiments and drawings, but the embodiments are not intended to limit the present invention.

[0020] The purpose of the present invention is to meet the needs of efficient, defect-free and high-quality friction stir welding of medium-thick high-strength titanium alloys with a thickness of more than 6 mm, and to provide a defect control method for friction stir welding of medium-thick plate titanium alloys, which can effectively broaden the process window, reduce welding defects, and reduce welding tool wear, thereby achieving high-quality friction stir welding of medium-thick high-strength titanium alloys.

[0021] In order to achieve the above object, the first aspect of the present invention provides a titanium alloy friction stir welding defect control method, comprising the following steps: The workpiece to be welded is heated by an auxiliary heat source arc, and when the workpiece reaches a plastic state, a stirring pin is inserted for penetration welding; during welding, the arc is placed in front to heat the metal to be welded in front of the stirring pin; Use positive and back gas protection to protect the molten pool and high temperature area after welding; Set the stirring needle length to be greater than the workpiece thickness; A back penetration forced forming groove is arranged at the back of the weld, the notch of the back penetration forced forming groove faces the weld and is used to accommodate the semi-solid plastic metal stirred and extruded by the end of the stirring pin; the back penetration forced forming groove corresponds to the stirring pin; During the welding process, the stirring needle and the back penetration forced forming groove are relatively stationary, and the workpiece to be welded is moved between the stirring needle and the back penetration forced forming groove.

[0022] Among them, the inner cavity of the back penetration forced forming groove is an inverted conical cavity with a groove depth of 0.2-1mm, which fits the shape of the top of the stirring needle. The front of the groove is tightly attached to the position of the weld to be welded, and the center of the groove coincides with the center line of the weld.

[0023] The welding gun generating the auxiliary heat source arc is fixed on the stir friction welding equipment, and the spatial position of the tungsten electrode is adjusted by rotating the contraction sleeve and the telescopic rod; wherein, the arc adopts a tungsten electrode with a size of 5-10mm and a frustum design, and the top size of the frustum is 2-5mm, so as to obtain a defocused arc.

[0024] The surface of the stirring needle is provided with spiral side grooves with a spiral angle of 6-8° and grooves along the axis direction of the stirring needle.

[0025] The arc and the stirring needle are on the same welding axis, and the arc is located in front of the stirring needle welding path. The distance between the two is related to the welding power. When the welding power is greater than 500 watts, the distance between the two is greater than 5mm, otherwise the distance between the two is less than 5mm.

[0026] The protective gas used is argon with a purity of 99.999% and a flow rate of 10-30L / min.

[0027] In one embodiment, a defect control method for friction stir welding of medium and thick titanium alloy plates includes the following steps: (1) Welding system layout In order to completely avoid the formation of unwelded defects, the back arc preheating and penetrating welding method can be used. At this time, it is necessary to find a space that can be accommodated for the stirring needle that penetrates the workpiece, such as Figure 1Through-penetration welding is achieved by designing a welding tool with a stirring needle longer than the thickness of the workpiece, axial support is achieved by designing a back-through welding forced forming groove structure to replace the welding pad, and through-penetration friction stir welding is achieved by opening a hole in the center of the back-through welding forced forming groove to accommodate the semi-solid plastic metal stirred and extruded by the end of the stirring needle.

[0028] In this case, the pressure at the end of the stirring needle is significantly reduced, so the degree of friction and wear is greatly reduced. At the same time, since the length of the stirring needle can be much larger than the thickness of the workpiece, even if the stirring needle is worn, the length of the stirring needle can be ensured to be greater than the thickness of the workpiece for a long time, effectively avoiding the formation of unwelded defects, thereby ensuring the stability of the welding process and obtaining a stir friction welding joint with consistent performance.

[0029] The auxiliary heat source penetration stir friction welding method can be used to completely avoid unwelded defects while performing welding at a higher speed. It can effectively reduce the heat input during the welding process, reduce the impact of welding heat generation on the deterioration of the joint structure, and obtain high-quality and high-strength stir friction welded joints.

[0030] See also Figure 2 As shown, the cavity of the back penetration forced forming groove is an inverted conical cavity, the front of the groove is close to the position of the weld to be welded, and the center of the groove coincides with the center line of the weld. Specifically, the front of the groove is close to the position of the weld to be welded, the center of the groove coincides with the center line of the weld, and the axis of the groove coincides with the axis of the stirring head. The forced forming groove is fixed on the stationary frame beam through a tool, and the stirring head is arranged on a rotating spindle, and the rotating spindle is installed on the stationary frame beam, wherein the rotating spindle is driven to rotate by a driving mechanism and drives the stirring head to rotate. During the welding process, the forced forming groove and the stirring head remain relatively still, that is, the workpiece to be welded is moving, while the stirring head and the back penetration forced forming groove remain relatively still. The test plate to be welded is fixed on the fastening tool and moves relative to the stirring needle with the tool, thereby achieving effective welding. In addition, the forming groove is conical in shape with a groove depth of 0.2-1mm, which matches the shape of the top of the stirring needle, but the overall size is slightly larger than the size of the stirring needle. On the one hand, it provides back support for penetration welding, and on the other hand, it can effectively accommodate the plastic metal extruded by the stirring needle during penetration welding, avoiding thinning problems on the front side due to the escape of plastic metal.

[0031] (2) Welding tools Arc-assisted stirring welding equipment is used to achieve efficient and high-quality welding of medium and thick titanium alloy plates. The auxiliary heat source arc welding gun is fixed on the stir friction welding equipment through the arc welding gun fixing device, and the spatial position of the tungsten electrode is adjusted by rotating the shrink sleeve and the telescopic rod. The arc adopts a large tungsten electrode and a truncated cone design to obtain a defocused arc, so that the welding material and the metal on the forward and backward sides of the stirring needle welding can be fully heated and softened. The tungsten electrode size is 5-10mm, and the top size of the truncated cone is 2-5mm.

[0032] Due to the heating effect of the auxiliary heat source, the titanium alloy reaches a semi-solid state and has good flow characteristics, so it is necessary to set a stirring head shape that increases flow. The surface of the stirring needle is designed with spiral side grooves with a helical angle of 6-8° and grooves along the axis of the stirring needle to increase the contact area between the stirring needle and the plate. Figure 3 As shown, the stirring needle designed with spiral side grooves 2 and grooves 1 can improve the flow filling ability of plastic metal, which helps to obtain a fully filled and defect-free welding joint.

[0033] (3) Welding process During welding, the back is first effectively heated to ensure that the weld metal reaches a plastic state, and then penetration welding is performed. When the stirring needle is inserted into the welding process, the arc is placed in front to heat the metal at the front of the stirring needle to be welded, reducing the strength of the material and improving the plasticity of the material, which is conducive to the subsequent stirring welding. The auxiliary heat source arc and the stirring needle are on the same welding axis. The auxiliary heat source arc is located in the front position of the stirring needle welding path. The distance between the two is related to the size of the welding power. When the welding power is greater than 500 watts, the distance between the two is greater than 5mm, otherwise the distance between the two is less than 5mm. During welding, the auxiliary heat source arc is preheated first, and stir friction welding begins after reaching above the recrystallization temperature of the titanium alloy. Welding protection is used throughout the welding process. Through the effective coupling of the auxiliary heat source arc and stir friction welding, efficient and high-quality stir friction welding of titanium alloys is achieved. The welding speed can reach more than 30mm / min, without welding defects, while ensuring that the joint tensile and impact toughness meet the use requirements.

[0034] (4) Welding protection During welding, the molten pool and the high temperature area after welding are protected by front and back gas protection. The protective gas flow rate is 10-30L / min, and the protective gas is argon with a purity of 99.999%.

[0035] A second aspect of the present invention provides a welded titanium alloy workpiece.

[0036] The third invention of the present invention provides an application of a welded titanium alloy workpiece in aircraft engines, flap rails, ships or marine engineering.

[0037] In order to further illustrate the defect control method for friction stir welding of medium and thick titanium alloy plates provided by the present invention, TC4 titanium alloy with a thickness of 6 mm is taken as an example for further explanation.

[0038] Example The present invention is used to weld TC4 titanium alloy with a thickness of 6 mm, and the steps are as follows: (1) Welding system layout The welding method of back arc preheating and penetrating the workpiece is adopted. At this time, it is necessary to find a space that can be accommodated for the stirring needle that penetrates the workpiece. Penetration welding is achieved by designing a welding tool with a stirring needle length greater than the thickness of the workpiece, and axial support is achieved by designing a back penetration forced forming groove structure to replace the welding pad. Penetration friction stir welding is achieved by opening a semi-solid plastic metal stirred and extruded by the end of the stirring needle in the center of the back penetration forced forming groove. In this case, the pressure at the end of the stirring needle is significantly reduced, so the degree of friction and wear is greatly reduced. At the same time, since the length of the stirring needle can be much greater than the thickness of the workpiece, even if the stirring needle is worn, it can also ensure that the length of the stirring needle is greater than the thickness of the workpiece for a long time, effectively avoiding the formation of unwelded defects, thereby ensuring the stability of the welding process and obtaining a stir friction welding joint with consistent performance.

[0039] The auxiliary heat source penetration stir friction welding method can be used to completely avoid unwelded defects while performing welding at a higher speed. It can effectively reduce the heat input during the welding process, reduce the impact of welding heat generation on the deterioration of the joint structure, and obtain high-quality and high-strength stir friction welded joints.

[0040] (2) Welding tools Arc-assisted stirring welding equipment is used to achieve efficient and high-quality welding of medium and thick titanium alloy plates. The auxiliary heat source arc welding gun is fixed on the stir friction welding equipment through the arc welding gun fixing device, and the spatial position of the tungsten electrode is adjusted by rotating the shrink sleeve and the telescopic rod. The arc adopts a large tungsten electrode and a truncated cone design to obtain a defocused arc, so that the welding material and the metal on the forward and backward sides of the stirring needle welding can be fully heated and softened. The tungsten electrode size is 6mm and the top size of the tungsten electrode truncated cone is 5mm.

[0041] Due to the heating effect of the auxiliary heat source, the titanium alloy reaches a semi-solid state and has good flow characteristics, so it is necessary to set a stirring head shape that increases flow. The surface of the stirring needle is designed with spiral side grooves with a helical angle of 7° and grooves along the axis of the stirring needle to increase the contact area between the stirring needle and the plate. Figure 3 As shown in the figure, the stirring needle with spiral side groove and groove design can improve the flow filling ability of plastic metal, which helps to obtain a fully filled and defect-free welding joint.

[0042] (4) Welding process During welding, the back is first effectively heated to ensure that the weld metal reaches a plastic state, and then penetration welding is performed. When the stirring needle is inserted into the welding process, the arc is placed in front to heat the metal at the front of the stirring needle to be welded, reducing the strength of the material and improving the plasticity of the material, which is conducive to the subsequent stirring welding. The auxiliary heat source arc and the stirring needle are on the same welding axis. The auxiliary heat source arc is located in the front position of the stirring needle welding path. The distance between the two is related to the size of the welding power. The welding power is 800 watts and the distance between the two is 10mm. During welding, the auxiliary heat source arc is preheated first, and stir friction welding begins after reaching above the recrystallization temperature of the titanium alloy. Welding protection is used throughout the welding process. Through the effective coupling of the auxiliary heat source arc and stir friction welding, efficient and high-quality stir friction welding of titanium alloys is achieved. The welding speed can reach more than 30mm / min without generating welding defects, while ensuring that the joint tensile strength and impact toughness meet the use requirements.

[0043] (4) Welding protection During welding, the molten pool and the high temperature area after welding are protected by front and back gas protection. The protective gas flow rate is 30L / min, and the protective gas is argon with a purity of 99.999%.

[0044] After welding, the welded joints were colored and X-rayed for nondestructive testing, which met the requirements of NB / T 47013 standard level I. No welding defects such as weak root bonding, unwelded head and tunnel were found. The performance of the welded joints was tested to obtain welded joints with good comprehensive performance. Among them, the tensile strength is 950MPa, which is as strong as the parent material, and the impact absorption energy of the weld can reach 49J, which meets the impact index of the welded joint.

Claims

1. A titanium alloy friction stir welding defect control method, characterized in that: The following steps are involved: The workpiece to be welded is heated by an auxiliary heat source arc, and when the workpiece reaches a plastic state, a stirring pin is inserted for penetration welding; during welding, the arc is placed in front to heat the metal to be welded in front of the stirring pin; Use positive and back gas protection to protect the molten pool and high temperature area after welding; Set the stirring needle length to be greater than the workpiece thickness; A back weld penetration forced forming groove is arranged at the back of the weld, the notch of the back weld penetration forced forming groove faces the weld, and the back weld penetration forced forming groove corresponds to the stirring pin; During the welding process, the stirring needle and the back penetration forced forming groove are relatively stationary, and the workpiece to be welded is moved between the stirring needle and the back penetration forced forming groove.

2. The titanium alloy friction stir welding defect control method according to claim 1, characterized in that: The inner cavity of the back penetration forced forming groove is an inverted conical cavity with a groove depth of 0.2-1mm, which matches the shape of the top of the stirring needle. The front of the groove is tightly attached to the position of the weld to be welded, and the center of the groove coincides with the center line of the weld.

3. The titanium alloy friction stir welding defect control method according to claim 1, characterized in that: The welding gun generating the auxiliary heat source arc is fixed on the stir friction welding equipment, and the spatial position of the tungsten electrode is adjusted by rotating the contraction sleeve and the telescopic rod; wherein, the arc adopts a tungsten electrode with a size of 5-10mm and a frustum design, and the top size of the frustum is 2-5mm, so as to obtain a defocused arc.

4. The titanium alloy friction stir welding defect control method according to claim 1, characterized in that: The surface of the stirring needle is provided with spiral side grooves with a spiral angle of 6-8° and grooves along the axis direction of the stirring needle.

5. The titanium alloy friction stir welding defect control method according to claim 1, characterized in that: The arc and the stirring needle are on the same welding axis, and the arc is located in front of the stirring needle welding path. The distance between the two is related to the welding power. When the welding power is greater than 500 watts, the distance between the two is greater than 5mm, otherwise the distance between the two is less than 5mm.

6. The titanium alloy friction stir welding defect control method according to claim 1, characterized in that: The protective gas used is argon with a purity of 99.999% and a flow rate of 10-30L / min.

7. A welded titanium alloy workpiece obtained by the method according to any one of claims 1 to 6.

8. Use of the welded titanium alloy workpiece according to claim 7 in aircraft engines, flap rails, aerospace, ships or marine engineering.

Citation Information

Patent Citations

  • Ultrasonic vibration aided stir friction welding process and device

    CN102744516B

  • Electromagnetic friction stir welding tools and methods

    CN103028838B

  • Friction stir welding technological method for conducting mobile heating on copper-aluminum dissimilar metal back face of thick plate

    CN108907448A

  • Supersonic vibration auxiliary friction stir welding device

    CN202726313U