A high-strength acrylate-modified silicone pressure-sensitive adhesive and preparation method thereof

By using multifunctional acrylate monomer and high-temperature crosslinking agent to form a 'soft-hard' interpenetrating network structure in acrylate modified silicone pressure-sensitive adhesive, it is solved that the bonding strength and heat resistance are difficult to synchronize in the prior art. The improvement problem has achieved high strength and stable pressure-sensitive adhesive performance, which is suitable for high-demand areas.

CN116042104BActive Publication Date: 2024-12-03INST OF PETROCHEM HEILONGJIANG ACADEMY OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310143862.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-21
Publication Date
2024-12-03
Estimated Expiration
2043-02-21

AI Technical Summary

Technical Problem

When the existing acrylate modified silicone pressure-sensitive adhesive improves bonding strength and heat resistance, the peel strength at room temperature will decrease. Due to the thermodynamic incompatibility of silicone and acrylate, the product performance is unstable and difficult to simultaneously Achieve high viscosity, peel strength and temperature resistance.

Method used

Using multifunctional acrylate monomer and high-temperature crosslinking agent, by forming a 'soft-hard' interpenetrating network structure and multiple crosslinking methods, combining carboxylic acrylate rubber and room temperature crosslinking agent to uniformly disperse the components and avoid phase Separation, improve crosslink density and synergistic effects.

Benefits of technology

It has achieved high-strength acrylate modified silicone pressure-sensitive adhesive, with high viscosity, peel strength and temperature resistance, and further improved performance after humidity and heat aging. It is suitable for high-demand areas such as aviation and aerospace.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004088456080000111
    Figure BDA0004088456080000111
  • Figure BDA0004088456080000121
    Figure BDA0004088456080000121
Patent Text Reader

Abstract

A high-strength acrylate-modified silicone pressure-sensitive adhesive and a preparation method thereof are intended to solve the problem that the existing silicone pressure-sensitive adhesive cannot have high holding force, peel strength and temperature resistance at the same time, and has poor resistance to moisture and heat aging. The pressure-sensitive adhesive comprises phenyl silicone rubber, MQ silicone resin, carboxyl acrylate rubber, difunctional acrylate monomer, trifunctional acrylate monomer, tetrafunctional acrylate monomer, pentafunctional acrylate monomer, room temperature crosslinking agent and high temperature crosslinking agent. Method: Add phenyl silicone rubber, MQ silicone resin, carboxyl acrylate rubber and mixed solvent to a reaction device, stir to obtain a basic adhesive solution; after cooling, add acrylate monomers and crosslinking agents of different functionalities in sequence, stir to obtain a modified adhesive solution; apply to the surface of a polyimide film to obtain a silicone pressure-sensitive adhesive. The pressure-sensitive adhesive of the present invention has high holding force and peel strength at the same time, and has excellent bonding performance and moisture and heat resistance at high temperature. The present invention is used to prepare silicone pressure-sensitive adhesive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of pressure-sensitive adhesives, and in particular to an acrylate-modified organic silicon pressure-sensitive adhesive and a preparation method thereof. Background Art

[0002] Pressure-sensitive adhesive is a type of adhesive that is sensitive to pressure and is widely used in packaging, labeling, electrical insulation, medical and health care, and honeycomb cutting and positioning. Among them, silicone pressure-sensitive adhesive, as a special pressure-sensitive adhesive material, has excellent properties such as high and low temperature resistance, UV resistance, and moisture resistance, and also has good adhesion to low surface energy materials such as polytetrafluoroethylene and silicone rubber. Silicone pressure-sensitive adhesive is mainly composed of silicone rubber, silicone resin, solvent, cross-linking agent and other additives. Acrylic pressure-sensitive adhesive has no unsaturated bonds in the main chain and has excellent antioxidant, weather resistance, oil resistance, medium resistance and high bonding strength. This type of pressure-sensitive adhesive is mainly prepared by copolymerization of soft monomers, hard monomers and a small amount of functional monomers, and has pressure sensitivity without the addition of tackifiers. Combining silicone and acrylate can obtain a modified pressure-sensitive adhesive product that has both excellent properties.

[0003] In the prior art, monofunctional acrylate monomers, vinyl-containing MQ silicone resins, etc. are used as raw materials to synthesize silicone-modified acrylate pressure-sensitive adhesives through copolymerization and other means. When the amount of silicone resin is 10%, the peel strength at room temperature is high, but the 180° peel strength at 150°C is less than 0.3N / mm. This technology uses acrylate as the main component, and the silicone component accounts for a small proportion, resulting in an insufficient temperature resistance level.

[0004] The modified pressure-sensitive adhesive is prepared by copolymerizing monofunctional acrylate monomers such as butyl acrylate, acrylic acid, 2-ethylhexyl acrylate, methyl methacrylate, acrylic acid, and hydroxyethyl acrylate with only 0.3-0.5% MQ silicone resin. The pressure-sensitive adhesive has a holding force of more than 24 hours and a 180° peel strength at room temperature of 0.2-0.32N / mm. This technology increases the holding force and heat resistance of the pressure-sensitive adhesive by increasing the cross-linking density through a single cross-linking method, but at the expense of the 180° peel strength at room temperature, it is impossible to achieve a simultaneous improvement in the bonding performance and heat resistance.

[0005] Another document reported a silicone-modified acrylate pressure-sensitive adhesive, which was obtained by free radical solution polymerization of vinyl silicone resin with unsaturated bonds and acrylate monomers. After 1000 hours of wet heat aging at 60°C, the 180° peel strength of the pressure-sensitive adhesive at room temperature was 0.23N / mm, which was significantly lower than that before aging. This shows that the pressure-sensitive adhesive with acrylate as the main component has relatively poor resistance to wet heat aging, and the peel strength will gradually decrease with the extension of aging time.

[0006] As can be seen from the above, in order to improve the bonding strength, the existing acrylate-modified silicone pressure-sensitive adhesive generally uses acrylate as the main component, and the silicone component accounts for a relatively small proportion. The temperature resistance level is not high enough, and the resistance to moisture and heat aging is relatively poor. The heat resistance of the pressure-sensitive adhesive is increased, but it is often at the expense of peel strength. At the same time, due to the thermodynamic incompatibility problem, silicone and acrylate are prone to phase separation, resulting in unstable performance of existing acrylate-modified silicone pressure-sensitive adhesive products. Therefore, it is difficult to produce acrylate-modified silicone pressure-sensitive adhesives with silicone as the main component. In addition, the single cross-linking method of acrylate-modified silicone pressure-sensitive adhesives and the uniform distribution of cross-linking points make it impossible to achieve the purpose of simultaneously improving bonding performance and heat resistance. Summary of the invention

[0007] The present invention aims to solve the problem that the existing organic silicon pressure-sensitive adhesive cannot have high holding force, peel strength and temperature resistance grade at the same time, and has poor resistance to wet heat aging, and provides a high-strength acrylate modified organic silicon pressure-sensitive adhesive and a preparation method thereof.

[0008] The invention provides a high-strength acrylate-modified organic silicone pressure-sensitive adhesive. The organic silicone pressure-sensitive adhesive comprises, by mass, 40-55 parts of phenyl silicone rubber, 40-80 parts of MQ silicone resin, 5-12 parts of carboxyl type acrylate rubber, 4-8 parts of difunctional acrylate monomer, 2-5 parts of trifunctional acrylate monomer, 0.5-2 parts of tetrafunctional acrylate monomer, 0.1-0.5 parts of pentafunctional acrylate monomer, 0.5-3 parts of room temperature crosslinking agent and 1-5 parts of high temperature crosslinking agent.

[0009] Furthermore, the molecular weight of the phenyl silicone rubber is 450,000 to 700,000, the phenyl content is 0.2 to 5.5%, and the vinyl content is 0.03 to 3.5%.

[0010] Furthermore, the M / Q ratio of the MQ silicone resin is (0.5-1.0):1, and the vinyl content is 0.2-5.8%.

[0011] Further, the difunctional acrylate monomer is 5-norbornene-2-methanol acrylate, polyethylene glycol diacrylate, ethylene glycol dimethacrylate, ethylene glycol diacrylate, 1,5-pentanediol diacrylate, diethylene glycol diacrylate, tetraethylene glycol diacrylate, dodecyl acrylate, 1,3-propylene glycol diacetate, tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, 1,3-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate, polyethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol diacrylate, 1,3-butanediol diacrylate, neopentyl glycol dimethacrylate, glycerol dimethacrylate. , neopentyl glycol diacrylate, 1,3-propylene glycol dimethacrylate, 1,6-di(acryloyloxy)-2,2,3,3,4,4,5,5-octafluorohexane, tetraethylene glycol dimethacrylate, 2-methyl-2-acrylic acid-1,12-dodecanol ester, 2-methyl-2-acrylic acid-1,10-decanediol ester, 2-methyl-2-acrylic acid-1,9-nonanediol ester, 1,3-dimethacrylate adamantyl ester, neopentyl glycol polymethyl ethylene oxide diacrylate, allyl diethylene glycol dicarbonate, 1,10-decanediol diacrylate, 1,4-butanediol diacrylate, polybutylene glycol diacrylate or 3-(acryloyloxy)-2-hydroxypropyl methacrylate.

[0012] Furthermore, the trifunctional acrylate monomer is trimethylolpropane triacrylate, ethoxylated trimethylolpropane triacrylate, pentaerythritol triacrylate, 1,1,1-trimethylol triacrylate, glycerol trihydroxypropyl ether triacrylate, 2,2',2"-nitrilotriethanol trimethacrylate or 1,1,1-trimethylol trimethacrylate.

[0013] Furthermore, the tetrafunctional acrylate monomer is pentaerythritol tetraacrylate or pentaerythritol tetramethacrylate.

[0014] Furthermore, the pentafunctional acrylate monomer is polydipentaerythritol pentaacrylate or sorbitol pentaacrylate.

[0015] Further, the room temperature crosslinking agent is pentaerythritol tris(3-aziridine)propionate, 6,7-bis(1-aziridine)-5,8-quinazolinedione, N,N-hexamethylene-1,6-bis(1-aziridineamide), N,N'-(methylenebis-P-phenyl)bis(aziridine-1-carboxamide), 1,1'-(1,3-phthaloyl)bis(2-methyl-aziridine), N-[4-[4-(aziridine-1-carbonylamino)-3-methylphenyl]-2-methylphenyl]aziridine-1-carboxamide, trimethylolpropane tris(2-methyl-1-aziridine propionate) or trimethylolpropane-tris(3-aziridine propionate).

[0016] Furthermore, the high temperature crosslinking agent is dibenzoyl peroxide, di-tert-butyl peroxide, di-tert-amyl peroxide, tert-butyl peroxybenzoate or 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane.

[0017] The method for preparing the above-mentioned high-strength acrylate-modified silicone pressure-sensitive adhesive comprises the following steps:

[0018] 1. Add 40-55 parts of phenyl silicone rubber, 40-80 parts of MQ silicone resin, and 5-12 parts of carboxyl type acrylate rubber into a reaction device, then add a mixed solvent to dissolve and dilute to a solid content of 35% to 40%, and stir at 110-125°C for 6-12h to obtain a basic glue solution; the mixed solvent is composed of toluene and ethyl acetate in a mass ratio of 3:1;

[0019] 2. Cool the basic glue obtained in step 1 to room temperature, add 4-8 parts of difunctional acrylate monomer, 2-5 parts of trifunctional acrylate monomer, 0.5-2 parts of tetrafunctional acrylate monomer, 0.1-0.5 parts of pentafunctional acrylate monomer, 0.5-3 parts of room temperature crosslinking agent and 1-5 parts of high temperature crosslinking agent in sequence, disperse and stir at room temperature until uniform and transparent, to obtain modified glue;

[0020] 3. Scrape the modified adhesive onto the surface of the polyimide film, let it stand at room temperature for 6 to 24 hours, then place it in an oven and heat it to 100°C and keep it for 40 to 60 minutes, then heat it to 150°C and keep it for 0.5 to 2 hours to obtain a high-strength acrylate-modified silicone pressure-sensitive adhesive.

[0021] Beneficial effects of the present invention:

[0022] The high-strength acrylate-modified organic silicon pressure-sensitive adhesive prepared by the invention has organic silicon as the main component, and carboxyl-type acrylate rubber, phenyl silicone rubber, MQ silicone resin and acrylate monomer are cross-linked in multiple ways, and the synergistic effect between different components is improved by forming a "soft-hard" interpenetrating network structure.

[0023] In the present invention, the "entanglement effect" of the carboxyl type acrylate rubber and the "anchoring effect" generated by the room temperature crosslinking agent and the carboxyl group are used to uniformly disperse acrylate monomers with different functionalities and the high temperature crosslinking agent in the pressure-sensitive adhesive system, thereby avoiding macroscopic phase separation during the high temperature crosslinking process. An acrylate-modified silicone pressure-sensitive adhesive with silicone as the main component is prepared, and the process is stable and suitable for large-scale production.

[0024] The co-introduction of difunctional acrylate monomer, trifunctional acrylate monomer, tetrafunctional acrylate monomer and pentafunctional acrylate monomer in the present invention further improves the crosslinking density of the system. Under the action of high-temperature crosslinking agent, the anchored acrylate monomers with different functionalities are chemically bonded with phenyl silicone rubber and MQ silicone resin. The local crosslinking point density formed by the low-functional acrylate monomer is small, and the local crosslinking point density formed by the high-functional acrylate monomer is large. The crosslinking point distribution in the overall space is uneven. This structure enables the pressure-sensitive adhesive system to maintain good plastic deformation ability while improving the crosslinking density, so that the prepared high-strength acrylate-modified silicone pressure-sensitive adhesive has the advantages of high holding force, peeling strength and high temperature resistance, and has excellent anti-wet heat aging performance. The holding force at 25°C is greater than 168h, the 180° peeling strength at 25°C is 1.58-1.92N / mm; the 180° peeling strength at 150°C is 0.47-0.68N / mm. After 1000h of heat aging at 70°C and 85% relative humidity, the 180° peel strength at 25°C is 1.73-2.16N / mm.

[0025] The pressure-sensitive adhesive prepared by the present invention can be applied to fields such as aviation and aerospace that require high holding force, high temperature resistance and high bonding strength. DETAILED DESCRIPTION

[0026] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any combination of the specific implementation modes.

[0027] Specific implementation method one: The high-strength acrylate-modified silicone pressure-sensitive adhesive of this implementation method includes, by mass, 40-55 parts of phenyl silicone rubber, 40-80 parts of MQ silicone resin, 5-12 parts of carboxyl-type acrylate rubber, 4-8 parts of difunctional acrylate monomer, 2-5 parts of trifunctional acrylate monomer, 0.5-2 parts of tetrafunctional acrylate monomer, 0.1-0.5 parts of pentafunctional acrylate monomer, 0.5-3 parts of room temperature crosslinking agent and 1-5 parts of high temperature crosslinking agent.

[0028] The high-strength acrylate-modified silicone pressure-sensitive adhesive prepared in this embodiment has silicone as the main component, and there are multiple cross-linking modes between carboxyl acrylate rubber, phenyl silicone rubber, MQ silicone resin, and acrylate monomers, which improves the synergy between different components by forming a "soft-hard" interpenetrating network structure.

[0029] Through the "entanglement effect" of carboxyl acrylate rubber and the "anchoring effect" produced by room temperature crosslinking agent and carboxyl group, acrylate monomers with different functionalities and high temperature crosslinking agent are evenly dispersed in the pressure-sensitive adhesive system, avoiding macroscopic phase separation during high temperature crosslinking process. Acrylate-modified silicone pressure-sensitive adhesive with silicone as the main component is obtained. The process is stable and can be suitable for large-scale production.

[0030] In this embodiment, the co-introduction of difunctional acrylate monomers, trifunctional acrylate monomers, tetrafunctional acrylate monomers and pentafunctional acrylate monomers further improves the crosslinking density of the system. Under the action of the high-temperature crosslinking agent, the anchored acrylate monomers with different functionalities are chemically bonded to the phenyl silicone rubber and MQ silicone resin. The local crosslinking point density formed by the low-functional acrylate monomers is small, and the local crosslinking point density formed by the high-functional acrylate monomers is large. The crosslinking point distribution in the overall space is uneven. This structure allows the pressure-sensitive adhesive system to maintain good plastic deformation ability while improving the crosslinking density, so that the prepared high-strength acrylate-modified silicone pressure-sensitive adhesive has the advantages of high holding force, peel strength and high temperature resistance, and also has excellent resistance to moisture and heat aging.

[0031] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that the molecular weight of the phenyl silicone rubber is 450,000 to 700,000, the phenyl content is 0.2 to 5.5%, and the vinyl content is 0.03 to 3.5%. Other aspects are the same as specific embodiment 1.

[0032] The introduction of a small amount of phenyl in the silicone rubber selected in this embodiment can improve the high temperature resistance of the pressure-sensitive adhesive while increasing the rigidity of the molecular chain, forming a "hard segment" cross-linking structure with the MQ silicone resin, and a "soft segment" cross-linking structure formed with the carboxyl type acrylate rubber and the room temperature cross-linking agent, thereby forming a "soft-hard" interpenetrating network structure and improving the synergistic effect between different components of the pressure-sensitive adhesive.

[0033] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that the M / Q ratio of the MQ silicone resin is (0.5-1.0):1, and the vinyl content is 0.2-5.8%. Other aspects are the same as specific implementation method 1 or 2.

[0034] The silicone resin selected in this embodiment has a moderate vinyl content, which ensures that the pressure-sensitive adhesive has appropriate cohesion through cross-linking reaction. If the vinyl content is too low, the pressure-sensitive adhesive cannot be effectively cross-linked, and if the vinyl content is too high, it will destroy the "uneven distribution of cross-linking points" of the acrylate monomer.

[0035] Specific embodiment 4: This embodiment is different from any of the specific embodiments 1 to 3 in that the difunctional acrylate monomer is 5-norbornene-2-methanol acrylate, polyethylene glycol diacrylate, ethylene glycol dimethacrylate, ethylene glycol diacrylate, 1,5-pentanediol diacrylate, diethylene glycol diacrylate, tetraethylene glycol diacrylate, dodecyl acrylate, 1,3-propylene glycol diacetate, tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, 1,3-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate, polyethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol diacrylate, 1,3-butanediol diacrylate, neopentyl dimethacrylate diol ester, glyceryl dimethacrylate, neopentyl glycol diacrylate, 1,3-propylene glycol dimethacrylate, 1,6-di(acryloyloxy)-2,2,3,3,4,4,5,5-octafluorohexane, tetraethylene glycol dimethacrylate, 2-methyl-2-acrylic acid-1,12-dodecanol ester, 2-methyl-2-acrylic acid-1,10-decanediol ester, 2-methyl-2-acrylic acid-1,9-nonanediol ester, 1,3-dimethacrylate adamantyl ester, neopentyl glycol polymethyl oxirane diacrylate, allyl diethylene glycol dicarbonate, 1,10-decanediol diacrylate, 1,4-butanediol diacrylate, polybutylene glycol diacrylate or 3-(acryloyloxy)-2-hydroxypropyl methacrylate. Others are the same as those in any one of the first to third embodiments.

[0036] Specific embodiment 5: This embodiment is different from any one of specific embodiments 1 to 4 in that the trifunctional acrylate monomer is trimethylolpropane triacrylate, ethoxylated trimethylolpropane triacrylate, pentaerythritol triacrylate, 1,1,1-trimethylol triacrylate, glycerol trihydroxypropyl ether triacrylate, 2,2',2"-nitrilotriethanol trimethacrylate or 1,1,1-trimethylol trimethacrylate. The rest is the same as any one of specific embodiments 1 to 4.

[0037] Specific embodiment 6: This embodiment is different from specific embodiments 1 to 5 in that the tetrafunctional acrylate monomer is pentaerythritol tetraacrylate or pentaerythritol tetramethacrylate. The rest is the same as specific embodiments 1 to 5.

[0038] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that the pentafunctional acrylate monomer is polydipentaerythritol pentaacrylate or sorbitol pentaacrylate. Other aspects are the same as those of specific embodiments 1 to 6.

[0039] Specific embodiment eight: This embodiment is different from any one of specific embodiments one to seven in that: the room temperature crosslinking agent is pentaerythritol tris (3-aziridine) propionate, 6,7-bis (1-aziridine) -5,8-quinazolinedione, N,N-hexamethylene-1,6-bis (1-aziridine amide), N,N'- (methylene bis-P-phenyl) bis (aziridine-1-carboxamide), 1,1'- (1,3-phthaloyl) bis (2-methyl-aziridine), N- [4- [4- (aziridine-1-carbonylamino) -3-methylphenyl] -2-methylphenyl] aziridine-1-carboxamide, trimethylolpropane tris (2-methyl-1-aziridine propionate) or trimethylolpropane-tris (3-aziridine propionate). Others are the same as any one of specific embodiments one to seven.

[0040] Specific embodiment 9: This embodiment is different from specific embodiments 1 to 8 in that the high temperature crosslinking agent is dibenzoyl peroxide, di-tert-butyl peroxide, di-tert-amyl peroxide, tert-butyl peroxybenzoate or 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane. Other aspects are the same as those of specific embodiments 1 to 8.

[0041] Specific embodiment 10: The preparation method of the high-strength acrylate-modified silicone pressure-sensitive adhesive in this embodiment comprises the following steps:

[0042] 1. Add 40-55 parts of phenyl silicone rubber, 40-80 parts of MQ silicone resin, and 5-12 parts of carboxyl type acrylate rubber into a reaction device, then add a mixed solvent to dissolve and dilute to a solid content of 35% to 40%, and stir at 110-125°C for 6-12h to obtain a basic glue solution; the mixed solvent is composed of toluene and ethyl acetate in a mass ratio of 3:1;

[0043] 2. Cool the basic glue obtained in step 1 to room temperature, add 4-8 parts of difunctional acrylate monomer, 2-5 parts of trifunctional acrylate monomer, 0.5-2 parts of tetrafunctional acrylate monomer, 0.1-0.5 parts of pentafunctional acrylate monomer, 0.5-3 parts of room temperature crosslinking agent and 1-5 parts of high temperature crosslinking agent in sequence, disperse and stir at room temperature until uniform and transparent, to obtain modified glue;

[0044] 3. Scrape the modified adhesive onto the surface of the polyimide film, let it stand at room temperature for 6 to 24 hours, then place it in an oven and heat it to 100°C and keep it for 40 to 60 minutes, then heat it to 150°C and keep it for 0.5 to 2 hours to obtain a high-strength acrylate-modified silicone pressure-sensitive adhesive.

[0045] The molecular weight of the phenyl silicone rubber is 450,000 to 700,000, the phenyl content is 0.2 to 5.5%, and the vinyl content is 0.03 to 3.5%. The M / Q ratio of the MQ silicone resin is (0.5 to 1.0): 1, and the vinyl content is 0.2 to 5.8%.

[0046] The difunctional acrylate monomer is 5-norbornene-2-methanol acrylate, polyethylene glycol diacrylate, ethylene glycol dimethacrylate, ethylene glycol diacrylate, 1,5-pentanediol diacrylate, diethylene glycol diacrylate, tetraethylene glycol diacrylate, dodecyl acrylate, 1,3-propylene glycol diacetate, tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, 1,3-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate, polyethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol diacrylate, 1,3-butanediol diacrylate, neopentyl glycol dimethacrylate, glycerol dimethacrylate, neopentyl glycol dimethacrylate, glycerol dimethacrylate, neopentyl glycol dimethacrylate, glycerol dimethacrylate, 1,3-butylene glycol diacrylate, 1,5-pentanediol diacrylate, 1,5-pentanediol diacrylate, 1,3-butylene glycol dimeth ... Pentylene glycol diacrylate, 1,3-propylene glycol dimethacrylate, 1,6-di(acryloyloxy)-2,2,3,3,4,4,5,5-octafluorohexane, tetraethylene glycol dimethacrylate, 2-methyl-2-acrylic acid-1,12-dodecanol, 2-methyl-2-acrylic acid-1,10-decanediol, 2-methyl-2-acrylic acid-1,9-nonanediol, 1,3-dimethacrylate adamantyl, neopentyl glycol polymethyl oxirane diacrylate, allyl diethylene glycol dicarbonate, 1,10-decanediol diacrylate, 1,4-butanediol diacrylate, polybutylene glycol diacrylate or 3-(acryloyloxy)-2-hydroxypropyl methacrylate.

[0047] The trifunctional acrylate monomer is trimethylolpropane triacrylate, ethoxylated trimethylolpropane triacrylate, pentaerythritol triacrylate, 1,1,1-trimethylol triacrylate, glycerol trihydroxypropyl ether triacrylate, 2,2',2"-nitrilotriethanol trimethacrylate or 1,1,1-trimethylol trimethacrylate.

[0048] The tetrafunctional acrylate monomer is pentaerythritol tetraacrylate or pentaerythritol tetramethacrylate.

[0049] The pentafunctional acrylate monomer is polydipentaerythritol pentaacrylate or sorbitol pentaacrylate.

[0050] The room temperature crosslinking agent is pentaerythritol tris (3-aziridine) propionate, 6,7-bis (1-aziridine) -5,8-quinazolinedione, N,N-hexamethylene-1,6-bis (1-aziridine amide), N,N'- (methylene bis-P-phenyl) bis (aziridine-1-carboxamide), 1,1'- (1,3-phthaloyl) bis (2-methyl-aziridine), N- [4- [4- (aziridine-1-carbonylamino) -3-methylphenyl] -2-methylphenyl] aziridine-1-carboxamide, trimethylolpropane tris (2-methyl-1-aziridine propionate) or trimethylolpropane-tris (3-aziridine propionate).

[0051] The high temperature crosslinking agent is dibenzoyl peroxide, di-tert-butyl peroxide, di-tert-amyl peroxide, tert-butyl peroxybenzoate or 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane.

[0052] The embodiments of the present invention are described in detail below. The following embodiments are implemented on the premise of the technical solution of the present invention, and detailed implementation schemes and specific operation processes are given, but the protection scope of the present invention is not limited to the following embodiments.

[0053] Embodiment 1:

[0054] The method for preparing the high-strength acrylate-modified silicone pressure-sensitive adhesive of this embodiment comprises the following steps:

[0055] 1. Add 40 parts of phenyl silicone rubber, 62 parts of MQ silicone resin and 6 parts of carboxyl type acrylate rubber into a conventional reaction device, then add a mixed solvent to dissolve and dilute to a solid content of 35%, and stir at 115°C for 10 hours to obtain a basic glue solution. The mixed solvent is composed of toluene and ethyl acetate in a mass ratio of 3:1.

[0056] 2. Cool the basic glue obtained in step 1 to room temperature, add 4.5 parts of polyethylene glycol diacrylate, 3 parts of pentaerythritol triacrylate, 0.8 parts of pentaerythritol tetraacrylate, 0.2 parts of polydipentaerythritol pentaacrylate, 1.6 parts of pentaerythritol tri(3-aziridinyl) propionate and 2.4 parts of dibenzoyl peroxide in sequence, disperse and stir at room temperature until uniform and transparent, to obtain a modified glue.

[0057] 3. Apply the modified glue to the surface of the polyimide film, let it stand at room temperature for 8 hours, then place it in an oven and heat it to 100°C for 40 minutes, then heat it to 150°C for 1.2 hours, and obtain 1 # High strength acrylate modified silicone pressure sensitive adhesive.

[0058] Among them, the molecular weight of the phenyl silicone rubber in step one is 520,000, the phenyl content is 5.3%, and the vinyl content is 0.21%; the M / Q ratio of the MQ silicone resin is 0.7:1, and the vinyl content is 2.7%.

[0059] Embodiment 2:

[0060] The difference between this embodiment and embodiment 1 is that:

[0061] The basic glue obtained in step 1 was cooled to room temperature, and 6 parts of tetraethylene glycol diacrylate, 2 parts of trimethylolpropane triacrylate, 1.3 parts of pentaerythritol tetraacrylate, 0.4 parts of polydipentaerythritol pentaacrylate, 2.4 parts of N,N-hexamethylene-1,6-bis(1-aziridine amide) and 1.5 parts of dibenzoyl peroxide were added in sequence, and dispersed and stirred at room temperature until it was uniform and transparent to obtain a modified glue. The other step parameters were the same as those in Example 1. Finally, 2 # High strength acrylate modified silicone pressure sensitive adhesive.

[0062] Embodiment 3:

[0063] The difference between this embodiment and embodiment 1 is that:

[0064] The basic glue obtained in step 1 was cooled to room temperature, and 6.5 parts of 1,6-hexanediol diacrylate, 4.5 parts of glycerol trihydroxypropyl ether triacrylate, 2 parts of pentaerythritol tetraacrylate, 0.1 parts of sorbitol pentaacrylate, 0.9 parts of 1,1'-(1,3-phthaloyl)bis(2-methyl-aziridine) and 3.5 parts of dibenzoyl peroxide were added in sequence, and the mixture was dispersed and stirred at room temperature until it became uniform and transparent to obtain a modified glue. The parameters of the other steps were the same as those in Example 1. Finally, 3 # High strength acrylate modified silicone pressure sensitive adhesive.

[0065] Embodiment 4:

[0066] The difference between this embodiment and embodiment 1 is that:

[0067] The basic glue obtained in step 1 was cooled to room temperature, and 8 parts of 1,3-butylene glycol diacrylate, 2.2 parts of 1,1,1-trimethylol trimethacrylate, 1.8 parts of pentaerythritol tetramethacrylate, 0.2 parts of sorbitol pentaacrylate, 0.6 parts of trimethylolpropane tris(2-methyl-1-aziridine propionate) and 2.4 parts of dibenzoyl peroxide were added in sequence, and the mixture was dispersed and stirred at room temperature until it became uniform and transparent to obtain a modified glue. The parameters of other steps were the same as those in Example 1. Finally, 4 # High strength acrylate modified silicone pressure sensitive adhesive.

[0068] Embodiment 5:

[0069] The method for preparing the high-strength acrylate-modified silicone pressure-sensitive adhesive of this embodiment comprises the following steps:

[0070] 1. Add 52 parts of phenyl silicone rubber, 75 parts of MQ silicone resin, and 10 parts of carboxyl acrylate rubber into a conventional reaction device, dissolve and dilute them with a mixed solvent of toluene: ethyl acetate in a mass ratio of 3:1 to a solid content of 38%, and stir at 115°C for 8 hours to obtain a basic glue solution.

[0071] 2. Cool the reaction product of step 1 to room temperature, add 7.2 parts of tetraethylene glycol dimethacrylate, 3.6 parts of 1,1,1-trimethylol ethyl triacrylate, 1.5 parts of pentaerythritol tetramethacrylate, 0.1 parts of sorbitol pentaacrylate, 2.5 parts of trimethylolpropane-tri(3-aziridinyl propionate) and 1.2 parts of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane in sequence, disperse and stir at room temperature until uniform and transparent to obtain a modified rubber solution.

[0072] 3. Apply the modified glue to the surface of the polyimide film, let it stand at room temperature for 18 hours, then place it in an oven and heat it to 100°C for 60 minutes, then heat it to 150°C for 2 hours to obtain 5 # High strength acrylate modified silicone pressure sensitive adhesive.

[0073] Among them, the molecular weight of the phenyl silicone rubber in step one is 520,000, the phenyl content is 5.3%, and the vinyl content is 0.21%; the M / Q ratio of the MQ silicone resin is 0.7:1, and the vinyl content is 2.7%.

[0074] Embodiment 6:

[0075] The difference between this embodiment and embodiment 5 is that:

[0076] 1. Add 48 parts of phenyl silicone rubber, 68 parts of MQ silicone resin, and 8 parts of carboxyl acrylate rubber into a conventional reaction device, dissolve and dilute them with a mixed solvent of toluene: ethyl acetate in a mass ratio of 3:1 to a solid content of 40%, and stir at 115°C for 12 hours to obtain a basic glue solution.

[0077] Among them, the molecular weight of the phenyl silicone rubber in step one is 650,000, the phenyl content is 3.8%, and the vinyl content is 0.09%; the M / Q ratio of the MQ silicone resin is 0.9:1, and the vinyl content is 5.1%.

[0078] The other step parameters are the same as those in Example 5. Finally, 6 # High strength acrylate modified silicone pressure sensitive adhesive.

[0079] Embodiment 7:

[0080] The difference between this embodiment and embodiment 5 is that:

[0081] 48 parts of phenyl silicone rubber, 75 parts of MQ silicone resin and 9 parts of carboxyl acrylate rubber were added into a conventional reaction device, dissolved and diluted with a mixed solvent of toluene:ethyl acetate in a mass ratio of 3:1 to a solid content of 38%, and stirred at 110°C for 12 hours to obtain a basic adhesive solution.

[0082] Among them, the molecular weight of the phenyl silicone rubber in step one is 650,000, the phenyl content is 3.8%, and the vinyl content is 0.09%; the M / Q ratio of the MQ silicone resin is 0.9:1, and the vinyl content is 5.1%.

[0083] The other step parameters are the same as those in Example 5. Finally, 7 # High strength acrylate modified silicone pressure sensitive adhesive.

[0084] Embodiment 8:

[0085] The difference between this embodiment and embodiment 5 is that:

[0086] Add 50 parts of phenyl silicone rubber, 75 parts of MQ silicone resin and 5 parts of carboxyl acrylate rubber into a conventional reaction device, dissolve and dilute them with a mixed solvent of toluene: ethyl acetate in a mass ratio of 3:1 to a solid content of 40%, and stir at 115°C for 10 hours to obtain a basic adhesive solution.

[0087] Among them, the molecular weight of the phenyl silicone rubber in step one is 520,000, the phenyl content is 2.6%, and the vinyl content is 1.7%; the M / Q ratio of the MQ silicone resin is 0.85:1, and the vinyl content is 1.4%.

[0088] The other step parameters are the same as those in Example 5. Finally, 8 # High strength acrylate modified silicone pressure sensitive adhesive.

[0089] Comparative Example 1: This example differs from Example 5 in that step 2:

[0090] The reaction product of step 1 was cooled to room temperature, and 7.2 parts of tetraethylene glycol dimethacrylate, 1.5 parts of pentaerythritol tetramethacrylate, 2.5 parts of trimethylolpropane-tri(3-aziridinyl propionate) and 1.2 parts of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane were added in sequence, and dispersed and stirred at room temperature until it became uniform and transparent to obtain a modified rubber solution.

[0091] The other step parameters are the same as those in Example 5. Finally, 9 # Acrylate modified silicone pressure sensitive adhesive.

[0092] Comparative Example 2: This example differs from Example 5 in that step 2:

[0093] The reaction product of step 1 was cooled to room temperature, and 0.2 parts of sorbitol pentaacrylate, 2.5 parts of trimethylolpropane-tri(3-aziridinyl propionate) and 1.2 parts of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane were added in sequence, and dispersed and stirred at room temperature until it became uniform and transparent to obtain a modified adhesive solution.

[0094] The other step parameters are the same as those in Example 5. Finally, 10 # Acrylate modified silicone pressure sensitive adhesive.

[0095] Comparative Example 3: This example differs from Example 5 in that step 2:

[0096] The reaction product of step 1 was cooled to room temperature, and 2.5 parts of trimethylolpropane-tri(3-aziridinyl propionate) and 1.2 parts of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane were added in sequence, and dispersed and stirred at room temperature until it became uniform and transparent to obtain a modified rubber solution.

[0097] The other step parameters are the same as those in Example 5. Finally, 11 # Acrylate modified silicone pressure sensitive adhesive.

[0098] Comparative Example 4: This example differs from Example 5 in that step 2:

[0099] The reaction product of step 1 was cooled to room temperature, and 7.2 parts of tetraethylene glycol dimethacrylate, 3.6 parts of 1,1,1-trimethylol ethyl triacrylate, 1.5 parts of pentaerythritol tetramethacrylate, 2.5 parts of trimethylolpropane-tri(3-aziridinyl propionate) and 1.2 parts of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane were added in sequence, and dispersed and stirred at room temperature until uniform and transparent to obtain a modified rubber solution.

[0100] The other step parameters are the same as those in Example 5. Finally, 12 # Acrylate modified silicone pressure sensitive adhesive.

[0101] The above 1 # ~12 # The pressure-sensitive adhesive was attached to LY12CZ aluminum alloy for bonding strength test. The holding force was tested according to GB / T4851-2014, and the 180° peel strength was tested according to GB / T 2792-2014. The test results are shown in Table 1.

[0102] As can be seen from Table 1, the high-strength acrylate-modified silicone pressure-sensitive adhesives of Examples 1 to 8 have high holding force, peel strength, temperature resistance and excellent resistance to wet heat aging. The holding force at 25°C is greater than 168h, the 180° peel strength at 25°C is 1.58-1.92N / mm; the 180° peel strength at 150°C is 0.47-0.68N / mm. After 1000h of wet heat aging at 70°C and 85% relative humidity, the 180° peel strength at 25°C is 1.73-2.16N / mm, which is slightly improved compared to before wet heat aging.

[0103] It can be seen from the data in Table 1 that without adding di-, tri-, tetra-, or pentafunctional acrylate monomers, or adding only one, two, or three of them, the prepared pressure-sensitive adhesive cannot have both high holding force and peel strength, and the 180° peel strength at high temperature and after wet heat aging is also relatively low.

[0104] Table 1

[0105]

[0106]

Claims

1. A high-strength acrylate-modified silicone pressure-sensitive adhesive, characterized in that The pressure-sensitive adhesive comprises 40-55 parts of phenyl silicone rubber, 40-80 parts of MQ silicone resin, 5-12 parts of carboxyl type acrylate rubber, 4-8 parts of difunctional acrylate monomer, 2-5 parts of trifunctional acrylate monomer, 0.5-2 parts of tetrafunctional acrylate monomer, 0.1-0.5 parts of pentafunctional acrylate monomer, 0.5-3 parts of room temperature crosslinking agent and 1-5 parts of high temperature crosslinking agent by weight; the molecular weight of the phenyl silicone rubber is 450,000-700,000, the phenyl content is 0.2-5.5%, and the vinyl content is 0.03-3.5%; the M / Q ratio of the MQ silicone resin is (0.5-1.0):1, and the vinyl content is 0.2-5.8%; the high temperature crosslinking agent is dibenzoyl peroxide, di-tert-butyl peroxide, di-tert-amyl peroxide, tert-butyl peroxybenzoate or 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane.

2. A high-strength acrylate-modified silicone pressure-sensitive adhesive according to claim 1, characterized in that: The difunctional acrylate monomer is polyethylene glycol diacrylate, ethylene glycol dimethacrylate, ethylene glycol diacrylate, 1,5-pentanediol diacrylate, diethylene glycol diacrylate, tetraethylene glycol diacrylate, tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, 1,3-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate, polyethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol diacrylate, 1,3-butanediol diacrylate, neopentyl glycol dimethacrylate, glycerol dimethacrylate, neopentyl glycol diacrylate, 1,3-propylene glycol diacrylate, 2-Methyl-2-acrylic acid-1,12-dodecanediol ester, 2-methyl-2-acrylic acid-1,10-decanediol ester, 2-methyl-2-acrylic acid-1,9-nonanediol ester, 1,3-dimethacrylate adamantyl ester, neopentyl glycol polymethyl oxirane diacrylate, allyl diethylene glycol dicarbonate, 1,10-decanediol diacrylate, 1,4-butanediol diacrylate, polybutylene glycol diacrylate or 3-(acryloyloxy)-2-hydroxypropyl methacrylate.

3. A high-strength acrylate-modified silicone pressure-sensitive adhesive according to claim 2, characterized in that: The trifunctional acrylate monomer is trimethylolpropane triacrylate, ethoxylated trimethylolpropane triacrylate, pentaerythritol triacrylate, 1,1,1-trimethylol triacrylate, glycerol trihydroxypropyl ether triacrylate, 2,2',2"-nitrilotriethanol trimethacrylate or 1,1,1-trimethylol trimethacrylate.

4. The high-strength acrylate-modified silicone pressure-sensitive adhesive according to claim 3, characterized in that: The tetrafunctional acrylate monomer is pentaerythritol tetraacrylate or pentaerythritol tetramethacrylate.

5. The high-strength acrylate-modified silicone pressure-sensitive adhesive according to claim 4, characterized in that: The pentafunctional acrylate monomer is polydipentaerythritol pentaacrylate or sorbitol pentaacrylate.

6. The high-strength acrylate-modified silicone pressure-sensitive adhesive according to claim 5, characterized in that: The room temperature crosslinking agent is pentaerythritol tris (3-aziridine) propionate, 6,7-bis (1-aziridine) -5,8-quinazolinedione, N,N-hexamethylene-1,6-bis (1-aziridine amide), N,N'- (methylene bis-P-phenyl) bis (aziridine-1-carboxamide), 1,1'- (1,3-phthaloyl) bis (2-methyl-aziridine), N- [4- [4- (aziridine-1-carbonylamino) -3-methylphenyl] -2-methylphenyl] aziridine-1-carboxamide, trimethylolpropane tris (2-methyl-1-aziridine propionate) or trimethylolpropane-tris (3-aziridine propionate).

7. The method for preparing a high-strength acrylate-modified silicone pressure-sensitive adhesive according to claim 1, characterized in that: The method comprises the following steps:

1. Add 40-55 parts of phenyl silicone rubber, 40-80 parts of MQ silicone resin, and 5-12 parts of carboxyl type acrylate rubber into a reaction device, then add a mixed solvent to dissolve and dilute to a solid content of 35% to 40%, and stir at 110-125°C for 6-12h to obtain a basic glue solution; the mixed solvent is composed of toluene and ethyl acetate in a mass ratio of 3:1; 2. Cool the basic glue obtained in step 1 to room temperature, add 4 to 8 parts of difunctional acrylate monomer, 2 to 5 parts of trifunctional acrylate monomer, 0.5 to 2 parts of tetrafunctional acrylate monomer, 0.1 to 0.5 parts of pentafunctional acrylate monomer, 0.5 to 3 parts of room temperature crosslinking agent and 1 to 5 parts of high temperature crosslinking agent in sequence, disperse and stir at room temperature until it is uniform and transparent to obtain a modified glue; the high temperature crosslinking agent is dibenzoyl peroxide, di-tert-butyl peroxide, di-tert-amyl peroxide, tert-butyl peroxybenzoate or 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane 3. Scrape the modified adhesive onto the surface of the polyimide film, let it stand at room temperature for 6 to 24 hours, then place it in an oven and heat it to 100°C and keep it for 40 to 60 minutes, then heat it to 150°C and keep it for 0.5 to 2 hours to obtain a high-strength acrylate-modified silicone pressure-sensitive adhesive.