Additive manufacturing method of particle reinforced metal matrix composite
The composite additive manufacturing method of arc fuse and laser powder feeding solves the problems of preparation efficiency and cost of particle-reinforced metal matrix composite materials in the existing technology, achieves efficient and low-cost molding and particle distribution uniformity, and improves the Properties of metal matrix composites.
Patent Information
- Application Number
- CN202410980320.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-22
AI Technical Summary
In the existing additive manufacturing of particle-reinforced metal matrix composites, selective laser additive manufacturing has low forming efficiency and difficulty in preparing large and complex parts, while arc fuse additive manufacturing has complex physical processes and many parameters, resulting in preparation efficiency and cost. Not good.
Using a composite method of arc fused wire additive manufacturing and laser powder feeding additive manufacturing, the metal is first cladded on the substrate through arc fused wire, and then laser cladded with particle reinforcement materials along the trajectory, combined with angle grinder grinding, layer by layer Reciprocating manufacturing, controlling the interlayer temperature to be less than 60°C, realizes the preparation of particle-reinforced metal matrix composite materials.
The preparation of particle-reinforced metal matrix composites with excellent molding, low cost and high efficiency is achieved, which saves particle reinforcement materials, reduces costs, and improves the mass fraction of reinforcement phase particles and the uniformity of material distribution.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of metal matrix composite materials and provides an additive manufacturing method for particle-reinforced metal matrix composite materials. Background Art
[0002] Metal matrix composites are new metal composites that are composed of metal or alloy as a matrix and one or more reinforcing phases. For particle-reinforced metal matrix composites, it is mainly based on aluminum, magnesium, and titanium as a matrix, and SiC, TiC, Si3N4, AlN, Al2O3, Y2O3, ZrO2, TiB2, etc. as particle reinforcement materials. Particle-reinforced metal matrix composites usually have higher specific stiffness and specific strength, making them highly competitive in comparison with conventional material performance.
[0003] Additive manufacturing technology is a new manufacturing technology in which the raw materials are heated to a molten state and deposited "layer by layer" along a predetermined thickness. Compared with traditional subtractive manufacturing and equal material manufacturing, it has the characteristics of low cost and high efficiency, and is widely used in the preparation of particle-reinforced metal matrix composites. At present, the additive manufacturing methods for preparing particle-reinforced metal matrix composites mainly include stir friction additive manufacturing technology, laser selective additive manufacturing and arc fuse additive manufacturing. Among them, stir friction additive manufacturing technology is a method of preparing metal matrix composites by rotating and hot pressing a stirring tool, and its flexibility is poor; laser additive manufacturing technology has the characteristics of no mold, low material consumption, short production cycle, and excellent forming quality, and is especially suitable for the forming of complex parts, but laser selective additive manufacturing of metal matrix composites has low forming efficiency and difficulty in preparing large and complex parts; arc fuse additive manufacturing technology has the advantages of high deposition rate, high material utilization rate and low equipment cost, but the physical process in arc additive manufacturing is complex and has many parameters, especially when wire is used as a filling material. At present, the wire preparation technology of particle-reinforced metal matrix composites still has great difficulties. Therefore, there is an urgent need to develop a preparation method that combines the excellent characteristics of laser additive manufacturing and the low cost and high efficiency characteristics of arc additive manufacturing and is suitable for metal matrix composites, so as to facilitate the preparation of metal matrix composites and promote the research of metal matrix composites and their application in production and life. Summary of the invention
[0004] In view of this, the present invention provides an additive manufacturing method for a particle-reinforced metal-based composite material to solve the problems existing in the prior art.
[0005] The present invention provides an additive manufacturing method for a particle-reinforced metal matrix composite material, comprising the following steps:
[0006] Step 1: polishing the substrate surface to remove the oxide film on the substrate surface, and then cleaning the polished substrate surface;
[0007] Step 2: Drying the metal wire and the reinforcement phase particle material separately;
[0008] Step 3: Using arc fuse additive manufacturing, a layer of metal is clad on the substrate using a high current and high voltage. After cladding, an angle grinder is used to grind to obtain an additive component with a preset metal cladding height;
[0009] Step 4: Using laser additive manufacturing, a layer of particle reinforcement material is clad on the additive component obtained in step 3 along the trajectory of arc fuse additive manufacturing, and after a period of time from the start of laser cladding, a layer of metal layer is clad on the particle reinforcement material along the trajectory of laser additive manufacturing by using arc fuse additive manufacturing. After cladding, an angle grinder is used for grinding to obtain a new additive component reaching a preset metal cladding height;
[0010] Step 5: Repeat step 4, control the interlayer temperature to be less than 60°C, and perform reciprocating additive manufacturing until the planned additive height is completed to obtain the final additive component.
[0011] Preferably, the preset metal cladding height is 8-10 mm; the particle reinforcement material cladding height is 1-2 mm.
[0012] More preferably, in step 4, the particle size of the particle reinforcement material is 1-100 μm.
[0013] Further preferably, in step 4, the speed of laser additive manufacturing is 300 mm / min-900 mm / min, and the powder feeding amount is 5-10 g / min.
[0014] Further preferably, in step 4, when the metal layer is clad by arc fuse additive manufacturing, the arc heat source is less than or equal to 20 mm from the laser heat source, and the temperature of the additive component is greater than 200°C.
[0015] Further preferably, in step four, the arc fuse additive speed is the same as the laser additive speed.
[0016] The additive manufacturing method of the particle reinforced metal matrix composite material provided by the present invention has excellent molding, low cost and high efficiency. The preparation of the particle reinforced metal matrix composite material can be achieved by combining arc fuse additive manufacturing and laser powder feeding additive manufacturing. That is, the metal matrix is prepared by arc additive manufacturing, and reinforcing particles are added between the layers of the metal matrix by laser powder feeding. While saving particle reinforcement materials, reducing costs and improving efficiency in the preparation process, the mass fraction of the reinforcing phase particles can be better controlled. DETAILED DESCRIPTION
[0017] The present invention will be further explained below in conjunction with specific implementation schemes, but the present invention is not limited thereto.
[0018] Laser powder feeding technology (laser additive manufacturing) is that when the powder of the reinforcing phase is ejected from the powder feeding nozzle through a carrier gas, the laser beam irradiates the substrate to form a liquid molten pool. After the powder interacts with the laser, as the powder feeding nozzle and the laser beam move synchronously, it enters the liquid molten pool and forms a cladding layer. The laser powder feeding system is simple to operate, has good cladding quality, easy to control penetration depth, and high laser utilization. Arc fuse technology is highly efficient, and wire preparation is easier than powder, and has great application value in the rapid prototyping of large parts. Therefore, the additive manufacturing technology combined with laser powder feeding and arc fuse used in the present invention has great advantages in the preparation of particle-reinforced metal-based composite materials.
[0019] The present invention provides an additive manufacturing method for a particle-reinforced metal matrix composite material, comprising the following steps:
[0020] Step 1: polishing the substrate surface to remove the oxide film on the substrate surface, and then cleaning the polished substrate surface;
[0021] Step 2: Drying the metal wire and the reinforcement phase particle material separately;
[0022] This step can avoid the generation of pores due to material moisture during the additive process;
[0023] Step 3: Using arc fuse additive manufacturing, a layer of metal is clad on the substrate using a high current and high voltage. After cladding, an angle grinder is used to grind to obtain an additive component with a preset metal cladding height;
[0024] In this step, the role of high current and high voltage is to firmly bond the additively manufactured material to the substrate, and to prevent the prepared material from being separated from the substrate due to stress caused by cladding;
[0025] Step 4: Using laser additive manufacturing, a layer of particle reinforcement material is clad on the additive component obtained in step 3 along the trajectory of arc fuse additive manufacturing, and after a period of time from the start of laser cladding, a layer of metal layer is clad on the particle reinforcement material along the trajectory of laser additive manufacturing by using arc fuse additive manufacturing. After cladding, an angle grinder is used for grinding to obtain a new additive component reaching a preset metal cladding height;
[0026] Step 5: Repeat step 4, control the interlayer temperature to be less than 60°C, and perform reciprocating additive manufacturing until the planned additive height is completed to obtain the final additive component.
[0027] Among them, the preset metal cladding height is 8-10mm; the particle reinforcement material cladding height is 1-2mm.
[0028] Wherein, in step 4, the particle size of the particle reinforcement material is 1-100 μm.
[0029] Among them, in step 4, the speed of laser additive is 300mm / min-900mm / min, and the powder feeding amount is 5-10g / min.
[0030] Among them, in step 4, when the metal layer is clad by arc fuse additive manufacturing, the arc heat source is less than or equal to 20 mm from the laser heat source, and the temperature of the additive component is greater than 200°C.
[0031] Among them, in step 4, the arc fuse additive speed is the same as the laser additive speed.
[0032] Example 1
[0033] The additive manufacturing method of TiB2 reinforced 2319 aluminum alloy, the specific implementation steps are as follows:
[0034] Step 1: Select an aluminum alloy plate with a size of 200*100*10mm as the substrate, grind the substrate surface by machining until the oil stains and aluminum oxide film on the substrate surface are removed, and then wipe the polished substrate surface with acetone;
[0035] Step 2: Drying aluminum wire (2319 aluminum wire with a diameter of 1.0 mm) and TiB2 particles (particle size of 10 μm) in a drying oven, wherein the drying temperature of the aluminum wire is 200° C., the holding time is 2 h, and the drying temperature of the TiB2 particles is 70° C., the holding time is 2 h;
[0036] Step 3: Through the method of arc fuse additive manufacturing, a layer of 2319 aluminum alloy is clad on the substrate using a large current and a large voltage to firmly bond the additive manufacturing material to the substrate. After cladding, an angle grinder is used to grind it. The cladding height is 8 mm. Pure argon is used as the shielding gas for arc fuse additive manufacturing. Under the protective atmosphere, the aluminum wire on the welding gun is heated by the arc to form a melt and enters the molten pool of the additive substrate along the direction of travel;
[0037] Step 4: Use laser as heat source to clad TiB2 particles on the aluminum alloy prepared in the previous step, with a cladding height of 1 mm, wherein the protective gas is 100% argon, and at a distance of 15 mm from the laser heat source, under a protective atmosphere, use an arc as a heat source to clad the aluminum alloy along the laser additive manufacturing track, and the aluminum wire on the welding gun is heated by the arc to form a melt and enter the molten pool, and mix with the TiB2 particles to form a TiB2-reinforced 2319-based composite material, wherein an angle grinder is used for grinding after cladding to make the metal cladding height of 8 mm, and the arc fuse additive speed is the same as the laser additive speed, both of which are 300 mm / min, and the powder feeding amount of the laser additive is 5 g / min;
[0038] Step 5: Repeat step 4, control the interlayer temperature to be less than 60°C, perform reciprocating additive manufacturing, and obtain components of TiB2 reinforced 2319-based composite materials.
[0039] Example 2
[0040] The additive manufacturing method of SiC reinforced Mg-9Al-1Si magnesium alloy has the following specific implementation steps:
[0041] Step 1: Select a magnesium alloy plate with a size of 200*100*10mm as the substrate, grind the substrate surface by machining until the oil stains and aluminum oxide film on the substrate surface are removed, and then wipe the polished substrate surface with acetone;
[0042] Step 2: Drying magnesium wire (Mg-9Al-1Si magnesium wire with a diameter of 1.0 mm) and SiC particles (particle size of 25 μm) in a drying oven, wherein the drying temperature of the magnesium wire is 120° C. and the holding time is 2 h, and the drying temperature of the SiC particles is 70° C. and the holding time is 2 h;
[0043] Step 3: Using the arc fuse additive manufacturing method, a layer of magnesium alloy is clad on the substrate using a large current and a large voltage to firmly bond the additive manufacturing material to the substrate. After cladding, an angle grinder is used to grind the material. The cladding height is 10 mm. Pure argon is used as the shielding gas for the arc fuse additive. Under the protective atmosphere, the magnesium wire on the welding gun is heated by the arc to form a melt and enters the molten pool of the additive substrate along the direction of travel;
[0044] Step 4: Using laser as a heat source, SiC particles are clad on the magnesium alloy prepared in the previous step, and the cladding height is 2 mm. The protective gas is 100% argon, and at a distance of 10 mm from the laser heat source, an arc is used as a heat source to clad the magnesium alloy along the laser additive manufacturing track under a protective atmosphere. The magnesium wire on the welding gun is heated by the arc to form a melt and enters the molten pool, where it is mixed with SiC particles to form a SiC-reinforced Mg-9Al-1Si magnesium-based composite material. After cladding, an angle grinder is used for grinding so that the metal cladding height is 10 mm. The arc fuse additive speed is the same as the laser additive speed, both of which are 900 mm / min, and the powder feeding amount of the laser additive is 10 g / min.
[0045] Step 5: Repeat step 4, control the interlayer temperature to be less than 60°C, perform reciprocating additive manufacturing, and obtain a component of SiC reinforced Mg-9Al-1Si magnesium-based composite material.
[0046] Example 3
[0047] The additive manufacturing method of WC reinforced maraging steel is implemented as follows:
[0048] Step 1: Select a martensitic steel plate with a size of 200*100*10mm as the substrate, grind the substrate surface by machining until the oil stains and aluminum oxide film on the substrate surface are removed, and then wipe the polished substrate surface with acetone;
[0049] Step 2: Drying the maraging steel wire (maraging steel wire with a diameter of 1.0 mm) and WC particles (particle size of 100 μm) in a drying oven, wherein the maraging steel wire is dried at a temperature of 120° C. for a holding time of 2 h, and the WC particles are dried at a temperature of 70° C. for a holding time of 2 h;
[0050] Step 3: Through the method of arc fuse additive manufacturing, a layer of martensitic aging steel is clad on the substrate using a large current and a large voltage to firmly bond the additive manufacturing material to the substrate. After cladding, an angle grinder is used for grinding. The cladding height is 9 mm. A mixed gas of 5% argon and 95% carbon dioxide is used as the shielding gas for arc fuse additive manufacturing. Under the protective atmosphere, along the direction of travel, the steel wire on the welding gun is heated by the arc to form a melt and enters the molten pool of the additive substrate;
[0051] Step 4: Using laser as heat source, WC particles are clad on the maraging steel prepared in the previous step, and the cladding height is 2 mm. The shielding gas is 100% argon gas, and at a distance of 20 mm from the laser heat source, under a protective atmosphere, an arc is used as a heat source to clad the magnesium alloy along the laser additive manufacturing track. The maraging steel wire on the welding gun is heated by the arc to form a melt and enters the molten pool, where it is mixed with the WC particles to form a WC reinforced maraging steel wire composite material. After cladding, an angle grinder is used for grinding to make the metal cladding height 9 mm. The arc fuse additive speed is the same as the laser additive speed, both of which are 500 mm / min, and the powder feeding amount of the laser additive is 8 g / min.
[0052] Step 5: Repeat step 4, control the interlayer temperature to be less than 60°C, perform reciprocating additive manufacturing, and obtain a component of a WC reinforced maraging steel wire composite material.
[0053] In Examples 1 to 3, particle-reinforced metal-based composite materials were successfully obtained, and the reinforced particles were relatively dispersed in the components without agglomeration. After testing, the metal-based composite materials prepared in this way have excellent performance, save particle reinforcement materials, reduce costs, improve efficiency, and can effectively control the mass fraction of the reinforcing phase particles.
Claims
1. A method for additive manufacturing of a particle-reinforced metal matrix composite material, characterized in that: The steps include: Step 1: polishing the substrate surface to remove the oxide film on the substrate surface, and then cleaning the polished substrate surface; Step 2: Drying the metal wire and the reinforcement phase particle material separately; Step 3: Using arc fuse additive manufacturing, a layer of metal is clad on the substrate using a large current and a large voltage. After cladding, an angle grinder is used to grind to obtain an additive component that reaches a preset metal cladding height; Step 4: Using laser additive manufacturing, a layer of particle reinforcement material is clad on the additive component obtained in step 3 along the trajectory of arc fuse additive manufacturing, and after a period of time from the start of laser cladding, a layer of metal layer is clad on the particle reinforcement material along the trajectory of laser additive manufacturing by using arc fuse additive manufacturing. After cladding, an angle grinder is used for grinding to obtain a new additive component reaching a preset metal cladding height; Step 5: Repeat step 4, control the interlayer temperature to be less than 60°C, and perform reciprocating additive manufacturing until the planned additive height is completed to obtain the final additive component.
2. The additive manufacturing method of the particle reinforced metal matrix composite material according to claim 1, characterized in that: The preset metal cladding height is 8-10mm; the particle reinforcement material cladding height is 1-2mm.
3. The additive manufacturing method of the particle reinforced metal matrix composite material according to claim 1, characterized in that: In step 4, the particle size of the particle reinforcement material is 1-100 μm.
4. The additive manufacturing method of the particle reinforced metal matrix composite material according to claim 1, characterized in that: In step 4, the speed of laser additive is 300mm / min-900mm / min, and the powder feeding amount is 5-10g / min.
5. The additive manufacturing method of the particle reinforced metal matrix composite material according to claim 1, characterized in that: In step 4, when the metal layer is clad by arc fuse additive manufacturing, the arc heat source is less than or equal to 20 mm from the laser heat source, and the temperature of the additive component is greater than 200°C.
6. The additive manufacturing method of the particle reinforced metal matrix composite material according to claim 1, characterized in that: In step 4, the arc fuse additive speed is the same as the laser additive speed.
Citation Information
Patent Citations
Electric arc and laser coaxial wire feeding and powder feeding printing spray head and additive manufacturing device
CN110587139A
Aluminum alloy plate surface laser cladding forming method
CN114381727A
Marine titanium alloy gradient composite material preparation method based on electric arc additive
CN114951689A
Method for improving surface forming precision of CMT electric arc additive manufacturing titanium alloy component
CN115958297A
Electric arc additive manufacturing metal matrix composite molten pool low-density particle floating effect restraining device and method
CN116532668A
Cited By
Aluminum-based composite material manufacturing device and method based on wire powder composite laser additive material
CN121972812A
Aluminum matrix composite manufacturing apparatus and method based on wire powder composite laser additive
CN121972812B