Composite silicon carbide fiber hard felt and preparation method thereof
Through potassium permanganate pretreatment and high-temperature treatment, combined with the formation of pyrolytic carbon interface layer and impregnation layer, the problem of traditional hard carbon felt being easily damaged at high temperatures is solved, and the thermal stability of composite silicon carbide fiber hard felt is significantly improved. stability and antioxidant properties.
Patent Information
- Application Number
- CN202411040810.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-31
AI Technical Summary
Traditional hard carbon felt is prone to structural damage under high temperatures and oxidizing environments, resulting in performance degradation and unable to meet the material performance requirements of modern industry.
Potassium permanganate is used to pretreat silicon carbide fibers to remove impurities on the fiber surface. Carbon fiber cloth and silicon carbide fiber cloth are alternately laid, high temperature treatment and composite densification are performed to form a pyrolytic carbon interface layer and impregnation layer to improve the material quality. thermal stability and antioxidant properties.
It significantly improves the thermal stability and mechanical properties of the composite silicon carbide fiber hard felt, enhances the overall structural strength and oxidation resistance of the material, and can maintain stable performance in harsh environments.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of composite fiber felt, and more specifically, to a composite silicon carbide fiber hard felt and a preparation method thereof. Background Art
[0002] As a high-performance composite material, carbon fiber hard felt is the most studied, most successfully applied and most widely used vacuum high-temperature thermal insulation material in the world. It is widely used in cemented carbide sintering furnaces, single crystal silicon furnaces, vacuum smelting furnaces, vacuum heat treatment furnaces, vapor deposition furnaces and other furnaces, and plays a vital role in energy conservation and emission reduction, and improving product grades. However, traditional hard carbon felt is mainly composed of a single carbon fiber or graphite fiber, and its structure is relatively simple and its performance is limited. Under high temperature and oxidizing environment, these materials are prone to structural damage, resulting in a rapid decline in performance, which cannot meet the growing demand of modern industry for material performance.
[0003] In order to solve the performance limitations of traditional hard carbon felt, researchers began to explore the development of new composite materials. Among them, silicon carbide ceramic fiber has become an ideal choice for improving the performance of hard carbon felt due to its excellent high temperature resistance, oxidation resistance and wear resistance. By compounding silicon carbide ceramic fiber with carbon fiber, hard carbon felt with higher performance stability can be prepared. However, it is prone to structural damage in high temperature and oxidative environments, resulting in performance degradation.
[0004] Therefore, how to prepare a composite silicon carbide fiber hard felt with good thermal stability is a problem that needs to be solved urgently. Summary of the invention
[0005] In order to improve the thermal stability of a composite silicon carbide fiber hard felt, the present application provides a composite silicon carbide fiber hard felt and a preparation method thereof.
[0006] In a first aspect, the present application provides a method for preparing a composite silicon carbide fiber hard felt, using the following technical solution: A method for preparing a composite silicon carbide fiber hard felt comprises the following preparation steps: (1) Pretreatment of silicon carbide fiber: immerse the silicon carbide fiber cloth in potassium permanganate with a mass concentration of 5-8% for 30-40 minutes, take it out, wash it, and dry it; (2) Preform molding: carbon fiber cloth and pretreated silicon carbide fiber cloth are alternately stacked and laid, and hot-pressed to obtain a silicon carbide / carbon fiber composite preform; (3) High temperature treatment: The prepared composite preform is heated to 1500-2500°C in a carbon monoxide atmosphere for high temperature treatment; (4) Composite densification: After the composite preform subjected to high temperature treatment is coated with a pyrolytic carbon layer, it is placed in an impregnating agent for immersion, and then taken out and subjected to high temperature carbonization to obtain the composite silicon carbide fiber hard felt.
[0007] By adopting the above technical scheme, potassium permanganate is used to pretreat silicon carbide fibers, which effectively removes impurities on the fiber surface, improves the purity of the fibers, improves the physical and chemical properties of the fibers, and to a certain extent improves the bonding force between the fibers and materials such as impregnants in subsequent operations, thereby improving the impregnation and deposition effects; the carbon fiber cloth and the silicon carbide fiber cloth are alternately stacked and arranged, and a preform with excellent layered structure and strength is prepared by hot pressing; high-temperature treatment is used to further improve the high-temperature structural stability of the preform, reduce the thermal stress of the fiber / matrix interface during the subsequent preform densification process, and possible defects such as pores and cracks are healed or eliminated at high temperatures, and the temperature is controlled at a high temperature of 1500-2500°C, which helps to increase the contact area between particles in the preform material, thereby accelerating the diffusion rate between atoms, which is beneficial to the bonding and sintering between fiber cloth layers, enhancing the overall structural strength of the preform, and improving the thermal stability of the preform.
[0008] A silicon-based impregnating agent is selected, which can form a protective layer on the surface of the preform, effectively blocking the corrosion of harmful substances such as oxygen and moisture in the external environment on the preform, thereby improving the heat resistance and oxidation resistance of the preform.
[0009] Optionally, the ratio of the number of layers of carbon fiber cloth to the number of layers of silicon carbide fiber cloth in the preform is 2:1.
[0010] By adopting the above technical solution, the combination of carbon fiber cloth and silicon carbide fiber cloth can complement each other's advantages and improve the comprehensive mechanical properties of the preform. Through a certain proportion of configuration, the advantages of high strength of carbon fiber cloth and high temperature resistance of silicon carbide fiber cloth can be fully utilized, thereby obtaining a preform with high overall strength and structural stability at high temperatures.
[0011] Optionally, during the preform forming operation, the temperature is raised to 150-180° C. at 12-15 MPa for hot pressing.
[0012] Optionally, the coating of the pyrolytic carbon interface layer adopts chemical vapor infiltration, using boron trichloride and methane as raw gas with a gas flow rate of 15 L / min, using nitrogen as carrier gas with a carrier gas flow rate of 30 L / min, and depositing at 900-1100°C for 2-3 hours.
[0013] By adopting the above technical solution, the uniform coating of the pyrolytic carbon layer is achieved. Boron trichloride and methane are used as raw gas. By controlling their gas flow, the reaction speed and coating thickness are accurately adjusted, so that the pyrolytic carbon interface layer can be evenly coated on the surface of the preform, thereby improving the performance of the preform. The pyrolytic carbon layer has excellent high temperature resistance, oxidation resistance and corrosion resistance, and can effectively protect the preform from erosion in harsh environments.
[0014] Optionally, the impregnation operation is to immerse the preform in an impregnating agent at a temperature of 140-170° C. and a pressure of 100-110 MPa for 20-30 minutes.
[0015] By adopting the above technical solution, under the action of temperature and pressure, the impregnating agent fully penetrates into the interior and surface of the preform, fills the tiny pores and defects in the preform, and makes the microstructure of the preform more dense and uniform.
[0016] Optionally, the silicon-based impregnating agent includes 8-10 parts of polysiloxane and 3-4 parts of carbon tetrachloride.
[0017] By adopting the above technical solution, polysiloxane contains silicon-oxygen bonds, which can undergo pyrolysis and carbonization reactions at high temperatures to form silicon carbide. At the same time, it has good permeability, and the added carbon tetrachloride further reduces the viscosity of the polysiloxane, helping the polysiloxane to be impregnated into the voids of the preform. At the same time, the carbon tetrachloride is volatilized and removed during the curing and carbonization process, and the remaining polysiloxane is converted into silicon carbide to enhance the density and uniformity of the hard felt, reduce the pores and defects inside it, and thus improve the thermal stability and mechanical properties of the hard felt.
[0018] Optionally, the high temperature carbonization operation is a heat treatment at 2200-2750° C. for 2-4 hours.
[0019] By adopting the above technical scheme, the impregnation layer is cured at 2200-2750°C, and the organic components in the preform are fully decomposed and carbonized. During the high-temperature carbonization process, the carbon atoms in the preform are rearranged to form a more stable crystal structure, eliminating internal residual stress and defects, optimizing the microstructure, and improving the ability of the hard felt to maintain stable performance in harsh working environments.
[0020] In the second aspect, the present application provides a composite silicon carbide fiber hard felt prepared by the method of the present application, comprising a silicon carbide / carbon fiber soft felt preform and a pyrolytic carbon interface layer and an impregnation layer sequentially coated on the surface of the preform; in the silicon carbide / carbon fiber soft felt preform, every two layers of carbon fiber felt layers have at least one silicon carbide fiber cloth layer, the carbon fiber felt layers and silicon carbide fiber cloth layers are alternately arranged, and both sides are carbon fiber felt layers.
[0021] In summary, this application has the following beneficial effects: 1. Since the present application adopts silicon carbide fiber and carbon fiber to composite to obtain a composite hard felt having the advantages of both carbon fiber and silicon carbide fiber, it has the advantages of high strength and good thermal stability.
[0022] 2. In this application, potassium permanganate is used to pretreat silicon carbide fiber cloth to help remove impurities on the fiber surface, improve fiber purity and uniformity, improve the overall performance of the fiber, reduce defects and stress concentration that may occur during high-temperature treatment, and promote the structural transformation of the crystals inside the fiber in coordination with high-temperature treatment, thereby improving the strength and toughness of the fiber, thereby improving the mechanical properties and high-temperature stability of the composite hard felt.
[0023] 3. A specific impregnating agent is used in this application. With the help of carbon tetrachloride, polysiloxane can better penetrate into the pores of the composite preform, fill and solidify, thereby reducing the pores and defects in the material and enhancing the strength of the entire structure. At the same time, the silicon element in the impregnating agent can effectively react with oxygen to form a dense oxide protective layer, organize oxygen corrosion on the preform, and help improve the material's antioxidant properties. DETAILED DESCRIPTION
[0024] The present application is further described in detail below with reference to the embodiments.
[0025] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0026] Polysiloxane was purchased from Jiangsu Rayne Environmental Protection Technology Co., Ltd., CAS: 63148-62-9; carbon fiber cloth used was Toray 12K-T700SC, with a tensile strength of 3400 MPa and a linear density of 1.8 g / cm 3 ; Silicon carbide fiber cloth was purchased from Forsman Technology (Beijing) Co., Ltd., item number 1404011. Preparation Example
[0027] Preparation Example 1 A silicon-based impregnating agent, the preparation of which comprises the following steps: 8 kg of polysiloxane and 4 kg of carbon tetrachloride were put into a mixing container, and heated and stirred at 50° C. for 10 minutes to obtain the silicon-based impregnating agent.
[0028] Preparation Example 2 A silicon-based impregnating agent, the preparation of which comprises the following steps: 10 kg of polysiloxane and 3 kg of carbon tetrachloride were put into a mixing container, and heated and stirred at 50° C. for 10 minutes to obtain the silicon-based impregnating agent. Example Example 1
[0029] A method for preparing a composite silicon carbide fiber hard felt, the preparation comprising the following steps: (1) Pretreatment of silicon carbide fiber: immerse the silicon carbide fiber cloth in a 5% potassium permanganate solution for 30 min, remove it, wash the unreacted solution with clean water, and dry it at 100°C; (2) Preform molding: Take carbon fiber cloth and pretreated silicon carbide fiber cloth and lay them alternately, first lay a layer of carbon fiber cloth, then lay a layer of silicon carbide fiber cloth on it, and then lay a layer of carbon fiber cloth, so that a layer of silicon carbide fiber cloth is sandwiched between the two layers of carbon fiber cloth, put it into a graphite mold, heat it to 150°C at 15MPa and keep it at a constant temperature for 30min, and hot press it to obtain a silicon carbide / carbon fiber composite preform. The size of the obtained silicon carbide / carbon fiber composite preform is 1000mm×1000mm×60mm; (3) High temperature treatment: The prepared composite preform is placed in a heating furnace, carbon monoxide is introduced, and the temperature is raised to 2000°C for high temperature treatment for 1 hour; (4) Composite densification: The composite preform after high-temperature treatment is placed in a chemical deposition furnace, and boron trichloride and methane are introduced. The added gas flow rate is controlled to be 15 L / min. Nitrogen is introduced as a carrier gas with a carrier gas flow rate of 30 L / min. After heating to 1100°C for deposition for 2 hours, it is taken out and cooled to room temperature. It is placed in the impregnating agent prepared in Preparation Example 1 and immersed for 20 minutes. The temperature during the impregnation process is controlled to be 160°C and the pressure is 100 MPa. After the impregnation is completed, it is taken out and high-temperature carbonized at 2200°C for 3 hours to obtain the composite silicon carbide fiber hard felt. Example 2
[0030] A method for preparing a composite silicon carbide fiber hard felt, the preparation comprising the following steps: (1) Pretreatment of silicon carbide fiber: immerse the silicon carbide fiber cloth in a potassium permanganate solution with a mass concentration of 8% for 30 minutes, remove it, wash the unreacted solution with clean water, and dry it at 100°C; (2) Preform molding: Take carbon fiber cloth and pretreated silicon carbide fiber cloth and lay them alternately, first lay a layer of carbon fiber cloth, then lay a layer of silicon carbide fiber cloth on it, and then lay a layer of carbon fiber cloth, so that a layer of silicon carbide fiber cloth is sandwiched between the two layers of carbon fiber cloth, put it into a graphite mold, heat it to 180°C at 12MPa and keep it at a constant temperature for 30min, and hot press it to obtain a silicon carbide / carbon fiber composite preform. The size of the obtained silicon carbide / carbon fiber composite preform is 1000mm×1000mm×60mm; (3) High temperature treatment: The prepared composite preform is placed in a heating furnace, carbon monoxide is introduced, and the temperature is raised to 1500°C for high temperature treatment for 1 hour; (4) Composite densification: The composite preform after high-temperature treatment is placed in a chemical deposition furnace, and boron trichloride and methane are introduced. The gas flow rate is controlled to be 15 L / min. Nitrogen is introduced as a carrier gas with a carrier gas flow rate of 30 L / min. After heating to 900°C for deposition for 2 hours, it is taken out and cooled to room temperature. It is placed in the impregnating agent prepared in Preparation Example 1 and immersed for 30 minutes. The temperature during the impregnation process is controlled to be 140°C and the pressure is 110 MPa. After the impregnation is completed, it is taken out and carbonized at 2400°C for 3 hours to obtain the composite silicon carbide fiber hard felt. Example 3
[0031] A method for preparing a composite silicon carbide fiber hard felt, the preparation comprising the following steps: (1) Pretreatment of silicon carbide fiber: immerse the silicon carbide fiber cloth in a 7% potassium permanganate solution for 30 min, remove it, wash the unreacted solution with clean water, and dry it at 100°C; (2) Preform molding: Take carbon fiber cloth and pretreated silicon carbide fiber cloth and lay them alternately, first lay a layer of carbon fiber cloth, then lay a layer of silicon carbide fiber cloth on it, and then lay a layer of carbon fiber cloth, so that a layer of silicon carbide fiber cloth is sandwiched between the two layers of carbon fiber cloth, put it into a graphite mold, heat it to 165°C at 13.5MPa and keep it at a constant temperature for 30min, and hot press it to obtain a silicon carbide / carbon fiber composite preform. The size of the obtained silicon carbide / carbon fiber composite preform is 1000mm×1000mm×60mm; (3) High temperature treatment: The prepared composite preform is placed in a heating furnace, carbon monoxide is introduced, and the temperature is raised to 2000°C for high temperature treatment for 1 hour; (4) Composite densification: The composite preform after high-temperature treatment is placed in a chemical deposition furnace, and boron trichloride and methane are introduced. The added gas flow rate is controlled to be 15 L / min. Nitrogen is introduced as a carrier gas with a carrier gas flow rate of 30 L / min. After heating to 1000°C for deposition for 3 hours, it is taken out and cooled to room temperature. It is placed in the impregnating agent prepared in Preparation Example 1 and immersed for 30 minutes. The temperature during the impregnation process is controlled to be 165°C and the pressure is 110 MPa. After the impregnation is completed, it is taken out and high-temperature carbonized at 2750°C for 3 hours to obtain the composite silicon carbide fiber hard felt. Example 4
[0032] A method for preparing a composite silicon carbide fiber hard felt, which is different from Example 1 in that the impregnating agent prepared in Preparation Example 2 is used in this embodiment. Example 5
[0033] A method for preparing a composite silicon carbide fiber hard felt, which is different from Example 1 in that the impregnating agent used in this example is not diluted with carbon tetrachloride. Comparative Example
[0034] Comparative Example 1 A method for preparing a composite silicon carbide fiber hard felt, which is different from Example 1 in that high temperature treatment is not performed in this comparative example, and the preparation steps are as follows: A method for preparing a composite silicon carbide fiber hard felt, the preparation comprising the following steps: (1) Pretreatment of silicon carbide fiber: immerse the silicon carbide fiber cloth in a 5% potassium permanganate solution for 30 min, remove it, wash the unreacted solution with clean water, and dry it at 100°C; (2) Preform molding: Take carbon fiber cloth and pretreated silicon carbide fiber cloth and lay them alternately, first lay a layer of carbon fiber cloth, then lay a layer of silicon carbide fiber cloth on it, and then lay a layer of carbon fiber cloth, so that a layer of silicon carbide fiber cloth is sandwiched between the two layers of carbon fiber cloth, put it into a graphite mold, heat it to 150°C at 15MPa and keep it at a constant temperature for 30min, and hot press it to obtain a silicon carbide / carbon fiber composite preform. The size of the obtained silicon carbide / carbon fiber composite preform is 1000mm×1000mm×60mm; (3) Composite densification: The above silicon carbide / carbon fiber composite preform is placed in a chemical deposition furnace, and boron trichloride and methane are introduced. The added gas flow rate is controlled to be 15 L / min. Nitrogen is introduced as a carrier gas with a carrier gas flow rate of 30 L / min. After heating to 1100°C and depositing for 2 hours, it is taken out and cooled to room temperature. It is placed in the impregnating agent prepared in Preparation Example 1 and immersed for 20 minutes. The temperature during the impregnation process is controlled to be 160°C and the pressure is 100 MPa. After the impregnation is completed, it is taken out and high-temperature carbonized at 2200°C for 3 hours to obtain the composite silicon carbide fiber hard felt.
[0035] Comparative Example 2 A method for preparing a composite silicon carbide fiber hard felt, which is different from Example 1 in that the high temperature treatment in this comparative example is performed after coating the pyrolytic carbon layer, and the preparation steps are as follows: A method for preparing a composite silicon carbide fiber hard felt, the preparation comprising the following steps: (1) Pretreatment of silicon carbide fiber: immerse the silicon carbide fiber cloth in a potassium permanganate solution with a mass concentration of 5-8% for 30 minutes, remove it, wash the unreacted solution with clean water, and dry it at 100°C; (2) Preform molding: Take carbon fiber cloth and pretreated silicon carbide fiber cloth and lay them alternately, first lay a layer of carbon fiber cloth, then lay a layer of silicon carbide fiber cloth on it, and then lay a layer of carbon fiber cloth, so that a layer of silicon carbide fiber cloth is sandwiched between the two layers of carbon fiber cloth, put it into a graphite mold, heat it to 150°C at 15MPa and keep it at a constant temperature for 30min, and hot press it to obtain a silicon carbide / carbon fiber composite preform. The size of the obtained silicon carbide / carbon fiber composite preform is 1000mm×1000mm×60mm; (3) Composite densification: The composite preform that has been subjected to high temperature treatment is placed in a chemical deposition furnace, and boron trichloride and methane are introduced. The added gas flow rate is controlled to be 15 L / min, and nitrogen is introduced as a carrier gas. The carrier gas flow rate is 30 L / min. After heating to 1100°C for deposition for 2 hours, it is taken out, cooled to room temperature, placed in a heating furnace, and carbon monoxide is introduced. The temperature is raised to 2000°C and high temperature treatment is performed for 1 hour. After cooling to room temperature, it was placed in the impregnating agent prepared in Preparation Example 1 and immersed for 20 minutes. During the immersion process, the temperature was controlled to be 160°C and the pressure was 100 MPa. After the immersion was completed, it was taken out and carbonized at 2200°C for 3 hours to obtain the composite silicon carbide fiber hard felt.
[0036] Comparative Example 3 A method for preparing a composite silicon carbide fiber hard felt is different from Example 1 in that potassium permanganate is not used to pretreat the silicon carbide fiber in this comparative example. Performance testing Detection Methods
[0037] Bending strength test: refer to GB / T 40398.2-2021 "Test methods for carbon-carbon composite carbon materials Part 2: Bending performance test" to test the hard felt prepared in the examples and comparative examples; Antioxidation test: After weighing the prepared sample, put it into a high-temperature furnace preheated to 1500℃, use air as the oxidant, keep the temperature constant for 30 minutes, take out the sample and cool it, use a brush to sweep away the oxidized loose powder layer on the surface of the sample, weigh it and calculate the oxidation weight loss; Thermal stability: After weighing the prepared sample, keep it at 1500℃ for 5 minutes, then cool and heat it at room temperature for 5 minutes for 10 hours, then weigh it and calculate the weight loss rate.
[0038] Table 1 Test data
[0039] It can be seen from Examples 1-3 and Comparative Examples 1-2 and Table 1 that high-temperature treatment of the fibers in appropriate operating steps is beneficial to reducing the thermal stress at the interface during the densification process of the preform, eliminating possible defects such as pores and cracks therein, enhancing the overall structural strength of the preform, and improving its thermal stability.
[0040] Combining Examples 1-3 with Comparative Example 3 and Table 1, it can be seen that the experimental data of Examples 1-3 are better than those of Comparative Example 3, indicating that the silicon carbide fiber cloth pretreated with potassium permanganate can improve the bonding ability with the coating material in the later stage, avoid the coating from being oxidized and falling off, and the pretreated fiber has good stability and still has good antioxidant properties after cold and hot treatment.
[0041] It can be seen from Examples 1-4 and Table 1 that the impregnating agent prepared from polysiloxane and carbon tetrachloride can penetrate well into the small gaps in the preform, enhance the density and uniformity of the hard felt, and thus improve the thermal stability of the hard felt.
[0042] Combining Example 1 with Example 5 and Table 1, it can be seen that the various experimental data of Example 1 are better than those of Example 5, indicating that the use of carbon tetrachloride can help reduce the viscosity of polysiloxane, which is beneficial to improve the fluidity of polysiloxane, so that polysiloxane can be better impregnated into the voids of the preform, reduce internal voids, and help improve the thermal stability of the hard felt finally obtained.
[0043] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A method for preparing a composite silicon carbide fiber hard felt, characterized in that: The method comprises the following preparation steps: (1) Pretreatment of silicon carbide fiber: immerse the silicon carbide fiber cloth in potassium permanganate with a mass concentration of 5-8% for 30-40 minutes, take it out, wash it, dry it and set it aside; (2) Preform molding: carbon fiber cloth and pretreated silicon carbide fiber cloth are alternately stacked and laid, and hot-pressed to obtain a silicon carbide / carbon fiber composite preform; (3) High temperature treatment: The prepared composite preform is heated to 1500-2500°C in a carbon monoxide atmosphere for high temperature treatment; (4) Composite densification: After the composite prefabricated deposited pyrolytic carbon layer is treated at high temperature, it is placed in an impregnating agent for impregnation, and then taken out for high-temperature carbonization to obtain the composite silicon carbide fiber hard felt, wherein the impregnating agent is a silicon-based impregnating agent.
2. The method for preparing a composite silicon carbide fiber hard felt according to claim 1, characterized in that: The ratio of the number of carbon fiber cloth layers to the number of silicon carbide fiber cloth layers in the preform is 2:
1.
3. The method for preparing a composite silicon carbide fiber hard felt according to claim 1, characterized in that: In the preform forming operation, the temperature is raised to 150-180° C. at 12-15 MPa for hot pressing.
4. The method for preparing a composite silicon carbide fiber hard felt according to claim 1, characterized in that: The pyrolytic carbon interface layer is deposited by chemical vapor deposition, using boron trichloride and methane as raw gas with a gas flow rate of 15 L / min, using nitrogen as carrier gas with a carrier gas flow rate of 30 L / min, and depositing at 900-1100° C. for 2-3 hours.
5. The method for preparing a composite silicon carbide fiber hard felt according to claim 1, characterized in that: The impregnation operation is to immerse the preform in the impregnating agent, control the pressure to be 100-110 MPa at a temperature of 140-170° C., and immerse for 20-30 minutes.
6. The method for preparing a composite silicon carbide fiber hard felt according to claim 5, characterized in that: The silicon-based impregnating agent comprises 8-10 parts of polysiloxane and 3-4 parts of carbon tetrachloride.
7. The method for preparing a composite silicon carbide fiber hard felt according to claim 1, characterized in that: The high temperature carbonization operation is a heat treatment at 2200-2750° C. for 2-4 hours.
8. A composite silicon carbide fiber hard felt prepared by the preparation method as described in any one of claims 1 to 7, comprising a silicon carbide / carbon fiber soft felt preform and a pyrolytic carbon interface layer and an impregnation layer sequentially coated on the surface of the preform; in the silicon carbide / carbon fiber soft felt preform, every two layers of carbon fiber felt layers have at least one silicon carbide fiber cloth layer, the carbon fiber felt layers and silicon carbide fiber cloth layers are alternately arranged, and both sides are carbon fiber felt layers.
Citation Information
Patent Citations
High-purity carbon fiber reinforced silicon carbide composite material and preparation method thereof
CN110105075A
Preparation method of thermal insulation hard felt for silicon carbide single crystal growth furnace
CN114213135A
Composite silicon carbide fiber hard felt as well as preparation method and application thereof
CN114773077A