Calcium hydrogen phosphate and preparation method thereof

By using nano-active calcium carbonate to react with phosphoric acid to control its crystal form and particle size, the problem of calcium carbonate residue and bubbles in the preparation of calcium hydrogen phosphate is solved, and the whiteness and use effect of the product are improved.

CN118851116APending Publication Date: 2024-10-29ZHENGZHOU RUIPU BIOLOGICAL ENG CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410995894.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

In the existing calcium hydrogen phosphate preparation process, residual calcium carbonate causes bubbles in the product, which affects the use effect and the product has low whiteness.

Method used

Using nano-active calcium carbonate as the calcium source, it reacts with phosphoric acid. By controlling the crystal form, particle size and moisture of nano-active calcium carbonate, its surface activity is improved to ensure that calcium carbonate and phosphoric acid fully react, avoid calcium carbonate residue, and prepare high-quality of calcium hydrogen phosphate.

Benefits of technology

It significantly reduces the gas production of calcium hydrogen phosphate products during use, improves the whiteness of the product, ensures the preparation of high-quality calcium hydrogen phosphate, and solves the problems of bubbles and low whiteness in traditional processes.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of calcium hydrogen phosphate preparation, in particular to calcium hydrogen phosphate and a preparation method thereof. The preparation method of the calcium hydrophosphate comprises the following steps: taking nano active calcium carbonate as a calcium source, and reacting with phosphoric acid to prepare the calcium hydrophosphate; the crystal form of the nano active calcium carbonate is cubic crystal form and / or fibrous, the particle size is 30-200nm, the moisture content is less than 6%, and the whiteness is more than 88%. According to the method, the nano active calcium carbonate is adopted as a calcium source, the crystal form, the particle size, the moisture and the whiteness of the nano active calcium carbonate are reasonably controlled, the surface activity of the calcium carbonate is improved, and the calcium carbonate can fully react with phosphoric acid during synthesis of calcium hydrogen phosphate, so that a high-quality calcium hydrogen phosphate product which is high in whiteness, less in gas production or free of bubbles is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of calcium hydrogen phosphate preparation, and in particular to calcium hydrogen phosphate and a preparation method thereof. Background Art

[0002] Phosphorus is an important element in organisms. It is used by organisms in the form of phosphate, so phosphate is an indispensable component in biological physiological processes. However, biological organisms cannot synthesize phosphates by themselves, and must be ingested through food or nutrients. The ingestion can be in the form of organic phosphates or inorganic phosphates. As a food additive, phosphate is widely used in various types of pasta, frozen foods, vegetable processing, canned foods, dairy products, wine, beverages and various types of baked foods such as bread and desserts abroad. The development speed of phosphate in my country has been relatively fast in the past 10 years, especially in recent years. As a food additive, the use and scope of phosphate are gradually expanding. At present, the most widely used variety of phosphate food additives in China is calcium hydrogen phosphate.

[0003] As a calcium salt in the form of orthophosphate, orthophosphate is the only phosphorus element that the body can absorb and utilize among many phosphates. At the same time, because calcium hydrogen phosphate is rich in calcium, it can help animals strengthen bone development and prevent osteoporosis, rickets, white diarrhea, paralysis and other diseases. Therefore, it has very important applications in the food industry. There are three functions of phosphate in food processing: one is to add it directly to food as a nutrient or nutritional enhancer; the second is to add it to food as a quality improver to improve food performance; the third is to improve the food processing process by using its special chemical structure. The role of calcium hydrogen phosphate in the food processing process is mainly in the first two aspects. As a safe nutritional enhancer, calcium hydrogen phosphate is mainly added to food to strengthen calcium intake, and can also be used to prevent or treat symptoms of calcium deficiency. At the same time, calcium hydrogen phosphate can also be used as an acidity regulator and pH buffer in food, and is used in milk powder, candy, pudding, condiments, meat additives and other foods.

[0004] At present, there are two main technologies for producing food-grade calcium hydrogen phosphate at home and abroad: the first is to neutralize phosphate rock powder with hydrochloric acid and lime milk, and then centrifuge, dry and crush to obtain calcium hydrogen phosphate products. This process has strict requirements on the content of the main raw materials. Phosphate rock powder needs to use high-grade phosphate rock, lime milk contains CaO>90%, and phosphoric acid contains high impurities. It is necessary to remove impurities during the production process and strictly control the pH value; this production process technology has low production costs, but the one-time investment is large, and it is suitable for large-tonnage continuous production. It is suitable for production near or near high-grade phosphate mines. The second is to neutralize food-grade phosphoric acid with calcium carbonate (calcium carbonate is generally obtained by crushing limestone by physical method), then centrifuge, dry and crush to obtain calcium hydrogen phosphate products. Although this production process is simple, the product whiteness is low, and bubbles appear in the product application. The reason for the bubbles is that the calcium carbonate used will have a large amount of residues during the reaction process, which is wrapped in the calcium hydrogen phosphate product, and then a large number of bubbles will appear when using calcium hydrogen phosphate.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The first object of the present invention is to provide a method for preparing calcium hydrogen phosphate, by using nano-active calcium carbonate as a calcium source, so that it can fully react with phosphoric acid when synthesizing calcium hydrogen phosphate, avoiding calcium carbonate residue during the reaction process and being wrapped in the calcium hydrogen phosphate product, thereby improving the gas generation problem of calcium hydrogen phosphate during use.

[0007] The second object of the present invention is to provide calcium hydrogen phosphate, which is prepared by the method for preparing calcium hydrogen phosphate as described above.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0009] A method for preparing calcium hydrogen phosphate comprises the following steps:

[0010] Nano-active calcium carbonate is used as a calcium source to react with phosphoric acid to produce calcium hydrogen phosphate;

[0011] The nanometer active calcium carbonate has a cubic crystal form and / or a fibrous form, a particle size of 30-200 nm, a moisture content of less than 6%, and a whiteness of more than 88%.

[0012] The method of the invention adopts nano-active calcium carbonate as a calcium source, and reasonably controls the crystal form, particle size, moisture and whiteness of the nano-active calcium carbonate, thereby improving the surface activity of the calcium carbonate so that the calcium carbonate can fully react with phosphoric acid during the synthesis of calcium hydrogen phosphate, thereby obtaining high-quality calcium hydrogen phosphate with high whiteness, less gas generation or no bubble generation.

[0013] A calcium hydrogen phosphate is prepared by the above-mentioned method for preparing calcium hydrogen phosphate.

[0014] The calcium hydrogen phosphate product provided by the invention has high whiteness, and compared with the calcium hydrogen phosphate prepared by using common heavy calcium carbonate, the gas production during use is significantly reduced.

[0015] Compared with the prior art, the present invention has the following beneficial effects:

[0016] (1) The method of the present invention prepares calcium hydrogen phosphate by reacting nano-active calcium carbonate with phosphonic acid. The process is simple. Nano-active calcium carbonate is used as a calcium source and its crystal form, particle size, moisture and other parameters are reasonably controlled. The fineness of calcium carbonate is increased, the specific surface area, porosity and surface energy of calcium carbonate powder are enlarged, and the surface activity of calcium carbonate is improved, so that calcium carbonate can fully react with phosphoric acid during the synthesis of calcium hydrogen phosphate, and unreacted calcium carbonate is avoided in the generated calcium hydrogen phosphate product, thereby significantly reducing the gas production of the calcium hydrogen phosphate product during use.

[0017] (2) The calcium hydrogen phosphate product provided by the present invention has high whiteness and generates little or no bubbles during use. DETAILED DESCRIPTION

[0018] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0019] A first aspect of the present invention provides a method for preparing calcium hydrogen phosphate, comprising the following steps:

[0020] Nano-active calcium carbonate is used as a calcium source to react with phosphoric acid to produce calcium hydrogen phosphate;

[0021] The nanometer active calcium carbonate has a cubic crystal form and / or a fibrous form, a particle size of 30-200 nm, a moisture content of less than 6%, and a whiteness of more than 88%.

[0022] When traditional methods use calcium carbonate and phosphoric acid to react to prepare calcium hydrogen phosphate, heavy calcium carbonate is usually obtained by physically crushing limestone. The prepared calcium hydrogen phosphate product has low whiteness and produces a large number of bubbles when used. The reason for the bubbles is that a large amount of heavy calcium carbonate used will remain during the reaction and be wrapped in the calcium hydrogen phosphate product. When the calcium hydrogen phosphate is used, the calcium carbonate wrapped therein decomposes to produce carbon dioxide, resulting in a large number of bubbles.

[0023] The invention adopts nano-active calcium carbonate as a calcium source, increases the fineness of calcium carbonate, expands the specific surface area, porosity and surface energy of calcium carbonate powder, and improves the surface activity of calcium carbonate, so that calcium carbonate can fully react with phosphoric acid during the synthesis of calcium hydrogen phosphate, thereby obtaining a calcium hydrogen phosphate product with high whiteness and low gas generation during use.

[0024] The invention can significantly reduce the gas production of calcium hydrogen phosphate products when they are used by reasonably controlling parameters such as the crystal form, particle size and moisture content of nano-active calcium carbonate. The particle size of the nano-active calcium carbonate is controlled to be 30-200nm, and the moisture content is less than 6%. The prepared calcium hydrogen phosphate generates only a small amount of bubbles when it is used. Compared with the traditional calcium hydrogen phosphate prepared by using ordinary heavy calcium carbonate, the amount of bubbles generated when it is used is significantly reduced.

[0025] For cubic nano-active calcium carbonate, the particle size refers to the side length of the cubic crystal; for fibrous nano-active calcium carbonate, the particle size refers to the diameter of the fiber rod. The crystal form and particle size affect the specific surface area of ​​calcium carbonate. The larger the specific surface area, the more fully it reacts with phosphoric acid. By controlling the crystal form and particle size, the residual calcium carbonate in calcium hydrogen phosphate can be reduced, thereby improving the gas production performance of calcium hydrogen phosphate when used; for example, in different embodiments, the particle size of the nano-active calcium carbonate used can be any point value among 30nm, 40nm, 54nm, 60nm, 80nm, 98nm, 110nm, 160nm, 200nm, or a range value composed of any two point values.

[0026] The moisture content of the nano-activated calcium carbonate used also affects the gas production performance of the prepared calcium hydrogen phosphate. The lower the moisture content of the nano-activated calcium carbonate, the less gas the prepared calcium hydrogen phosphate produces during application. For example, in different embodiments, the moisture content of the nano-activated calcium carbonate used can be 0.15%, 2.36%, 5.69%, and the like.

[0027] The whiteness of the nano-activated calcium carbonate used mainly affects the whiteness of the prepared calcium hydrogen phosphate product. For example, in different embodiments, the whiteness of the nano-activated calcium carbonate used can be 88.4, 90.3, 92.6, and so on.

[0028] In some preferred embodiments of the present invention, the nano-active calcium carbonate has a cubic crystal form, a particle size of 30-100 nm, a moisture content of <2.5%, and a whiteness of ≥90. When the parameters of the nano-active calcium carbonate are controlled within this range, the prepared calcium hydrogen phosphate generates only a trace amount of bubbles when used, and the whiteness is also above 90.

[0029] In some more preferred embodiments of the present invention, the nano-active calcium carbonate has a cubic crystal form, a particle size of 30-60 nm, a moisture content of ≤0.5%, and the prepared calcium hydrogen phosphate generates no bubbles when used.

[0030] In some specific embodiments of the present invention, the method for preparing the nano-activated calcium carbonate comprises the following steps:

[0031] S1. CO2 gas is introduced into the calcium hydroxide suspension, and a crystal modifier is added to perform a carbonization reaction to obtain a calcium carbonate slurry;

[0032] S2. Add a surfactant to the calcium carbonate slurry for stirring and activation, solid-liquid separation, washing, and drying to obtain the nano-activated calcium carbonate.

[0033] The purpose of adding a crystal form regulator is to synthesize nano-scale calcium carbonate with a large specific surface area and a cubic or fibrous crystal form. The role of adding a surfactant is to prevent the finer calcium carbonate particles from secondary agglomeration to form particles with larger secondary particle sizes. By adding a crystal form regulator and a surfactant, the crystal form and particle size of nano-active calcium carbonate can be controlled, thereby adjusting the gas production of the calcium hydrogen phosphate product.

[0034] In some specific embodiments of the present invention, the mass concentration of the calcium hydroxide suspension is 20%-30%, for example, any point value among 20%, 22%, 24%, 26%, 28%, 30% or a range value composed of any two values.

[0035] In some specific embodiments of the present invention, the temperature of the carbonization reaction is 30-60°C, for example, any point value among 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, and 60°C, or a range value composed of any two point values. The temperature of the carbonization reaction has a great influence on the particle size and whiteness of the generated calcium carbonate. The higher the carbonization temperature, the larger the particle size of the generated calcium carbonate and the lower the whiteness, which leads to a decrease in the content and whiteness of calcium hydrogen phosphate in the final product. In addition, the amount of bubbles generated by calcium hydrogen phosphate generated by calcium carbonate with a larger particle size during use will also increase. Therefore, the carbonization temperature needs to be reasonably controlled. In some specific embodiments, the heating method of the carbonization process is water bath heating.

[0036] In some specific embodiments of the present invention, in step S1, the step of carbonization reaction includes: firstly introducing CO2 gas to carbonize until the pH value of the slurry is 7-8, at which time the carbonization rate is 15%-30%, then adding the crystal form regulator, and then continuing to introduce CO2 gas to carbonize until the pH value of the slurry is 5-6, so as to obtain the calcium carbonate slurry.

[0037] The carbonation rate refers to the degree to which calcium hydroxide and carbon dioxide react to form calcium carbonate. pH paper is used to make judgments during actual operation.

[0038] In some specific embodiments of the present invention, during the entire carbonization process, the molar ratio of calcium hydroxide to CO2 is 1:3-3.1.

[0039] In some specific embodiments of the present invention, the crystal form regulator includes sulfuric acid and / or phosphoric acid.

[0040] When sulfuric acid is used as a crystal form regulator, the generated calcium carbonate is a cubic crystal form. In some specific embodiments of the present invention, sulfuric acid is usually prepared into a 5%-10% sulfuric acid solution and added; when phosphoric acid is used as a crystal form regulator, the generated calcium carbonate is a fibrous crystal form.

[0041] In some specific embodiments of the present invention, the amount of the crystal form regulator added is 1.0%-3.0% of the slurry weight, for example, any point value among 1.0%, 1.5%, 2.0%, 2.5%, 3.0% or a range value consisting of any two point values.

[0042] In some specific embodiments of the present invention, the surfactant includes at least one of 2-lauric acid glyceryl monoester, 2-myristic acid glyceryl monoester, and C15-C18 fatty acids.

[0043] In some preferred embodiments of the present invention, the surfactant includes 2-lauric acid glyceryl monoester and / or 2-myristic acid glyceryl monoester.

[0044] In some more preferred embodiments of the present invention, the surfactant includes 2-laurin monoglyceride.

[0045] In some specific embodiments of the present invention, the amount of the surfactant is 5%-10% by weight of calcium carbonate, for example, any value among 5%, 6%, 7%, 8%, 9%, 10% or a range consisting of any two values.

[0046] In some specific embodiments of the present invention, the surfactant is added in the form of a solution, and the preparation step of the surfactant solution includes: mixing the surfactant with water at 50-70°C, and fully stirring and dispersing to form a surfactant solution, wherein the water is preferably deionized water, and the preparation of the surfactant solution is carried out under heating conditions, and the heating can fully disperse the surfactant in the water.

[0047] In some specific embodiments of the present invention, the stirring activation temperature is 70-90°C, for example, any point value among 70°C, 75°C, 80°C, 85°C, and 90°C, or a range value consisting of any two point values, and the stirring activation time is 0.5-3.5h, for example, any point value among 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, and 3.5h, or a range value consisting of any two point values.

[0048] In some specific embodiments of the present invention, the washing includes water washing, the water washing temperature is 50-70° C., and the water washing time is 1-2 h.

[0049] The purpose of water washing is to remove impurity ions in calcium carbonate. The solubility of sulfate is maximum at 60°C. When sulfuric acid is used as a crystal form regulator, washing with deionized water at 50-70°C can effectively remove sulfate impurities.

[0050] In some specific embodiments of the present invention, during water washing, the mass ratio of the wet material to deionized water is 1:4-4.1.

[0051] In some specific embodiments of the present invention, the drying temperature is 150-230°C, for example, any point value among 150°C, 160°C, 170°C, 180°C, 200°C, and 230°C, or a range value consisting of any two point values; the drying time is 16-20h, for example, any point value among 16h, 17h, 18h, 19h, and 20h, or a range value consisting of any two point values. By controlling the drying conditions, the moisture content of nano-activated calcium carbonate is controlled within a certain range to avoid increased gas production during the use of the final product calcium hydrogen phosphate due to excessively high moisture content of calcium carbonate.

[0052] In some specific embodiments of the present invention, the method for preparing calcium hydrogen phosphate comprises the following steps:

[0053] The nano-active calcium carbonate is dispersed in water to prepare a calcium carbonate suspension; the calcium carbonate suspension is slowly added dropwise to a phosphoric acid solution, the pH is adjusted to 2.5-3.5, and the reaction is fully carried out; the pH is adjusted to 4-5 with a calcium hydroxide solution, and after the reaction is fully carried out, the calcium hydrogen phosphate is obtained through aging, solid-liquid separation, and drying.

[0054] In some specific embodiments of the present invention, the synthesis temperature of the calcium hydrogen phosphate is 30-50°C. The purpose of controlling the temperature is to ensure the crystal water content of calcium hydrogen phosphate dihydrate generated by the subsequent reaction. Too high a temperature will cause the calcium hydrogen phosphate dihydrate to lose its crystal water. The reaction time is: after the calcium carbonate suspension is added dropwise to the phosphoric acid solution to adjust the pH to 2.5-3.5, the reaction is continued for 1-2 hours; after the calcium hydroxide solution is used to adjust the pH to 4-5, the reaction is continued for 1-2 hours.

[0055] In some specific embodiments of the present invention, the mass concentration of the phosphoric acid solution is 35%-60%, for example, any point value among 35%, 40%, 45%, 50%, 55%, 60% or a range value consisting of any two point values.

[0056] In some specific embodiments of the present invention, the dropping speed of the calcium carbonate suspension is 5-10 mL / min, for example, any point value among 5 mL / min, 6 mL / min, 7 mL / min, 8 mL / min, 9 mL / min, 10 mL / min, or a range value consisting of any two point values, and the molar ratio of the nano-activated calcium carbonate to the phosphoric acid is 1:1.5-1.7, for example, any point value among 1:1.5, 1:1.6, 1:1.7, or a range value consisting of any two point values.

[0057] In some specific embodiments of the present invention, the aging temperature is 30-50°C, such as any point value among 30°C, 35°C, 40°C, 45°C, and 50°C, or a range consisting of any two fixed values, and the aging time is 2-3h, such as any point value among 2h, 2.5h, and 3h, or a range consisting of any two point values.

[0058] In some specific embodiments of the present invention, the drying temperature is 50-70°C, for example, any point value among 50°C, 55°C, 60°C, 65°C, and 70°C, or a range value consisting of any two point values, and the drying time is 1-2h, for example, any point value among 1h, 1.5h, and 2h, or a range value consisting of any two point values.

[0059] A calcium hydrogen phosphate is prepared by the method for preparing calcium hydrogen phosphate described in any one of the aforementioned embodiments.

[0060] The calcium hydrogen phosphate product provided by the invention has high whiteness and produces little gas during use.

[0061] The following is a detailed description of some embodiments of the present invention in conjunction with specific application examples. The raw materials used in the examples can be purchased from the market unless otherwise specified.

[0062] (I) The influence of nano-activated calcium carbonate and ordinary heavy calcium carbonate on the performance of calcium hydrogen phosphate:

[0063] Example 1

[0064] 1) Preparation of nano-activated calcium carbonate

[0065] S1. 500 mL of deionized water was measured in a 1 L beaker, 148 g of calcium hydroxide was slowly added, and the mixture was heated in a water bath at 35 ° C. The mixture was stirred thoroughly to obtain a calcium hydroxide suspension. CO2 gas was introduced into the calcium hydroxide suspension to cause carbonization reaction until the pH value of the slurry was 7-8. 13 g of a sulfuric acid solution having a mass concentration of 98% was added, and CO2 was continued to be introduced to carbonize the slurry until the pH value of the slurry was 5-6 to obtain a nano-scale cubic calcium carbonate slurry. The actual yield of calcium carbonate was about 90%.

[0066] S2. Measure 200 mL of deionized water in another 1L beaker, heat it in a water bath at 60°C, add 100 g of 2-lauric acid glycerol monoester, stir and disperse it in water to form a surfactant solution;

[0067] The calcium carbonate slurry prepared in step S1 was heated to 80°C in a water bath, 30g of surfactant solution was added, and the mixture was kept warm and stirred for 2h. The mixture was filtered using a Buchner funnel. After sufficient filtration, the wet calcium carbonate was added to 400ml of deionized water, washed with water at 60°C for 1.5h, filtered twice, and then dried in a forced air drying oven at 200°C for 18h to obtain nano-activated calcium carbonate.

[0068] 2) Preparation of calcium hydrogen phosphate

[0069] A. Measure 300 mL of deionized water in a 1 L beaker, add 70 g of nano-activated calcium carbonate synthesized by the above process, heat to 35°C, and stir thoroughly until the calcium carbonate is evenly dispersed in the water to obtain a calcium carbonate suspension.

[0070] B. Measure 200 mL of deionized water into another 1 L beaker, add 115.5 g of phosphoric acid, stir thoroughly, and heat in a 35°C water bath to obtain a phosphoric acid solution.

[0071] C. At 35°C, add the calcium carbonate suspension to the phosphoric acid solution at a rate of 8 mL / min, adjust the pH to about 3, and allow to react for 1.5 hours. Use calcium hydroxide solution to adjust the pH to 4-5, and stir the reaction for 1.5 hours.

[0072] D. The slurry after the reaction in step C is subjected to a aging treatment, and is aged in a water bath at 35° C. for 2.5 hours to obtain an aged calcium hydrogen phosphate slurry.

[0073] E. After the aging is completed, the slurry is filtered and dried, and dried in a forced air drying oven at 60° C. for 1.5 h to obtain the calcium hydrogen phosphate product.

[0074] Comparative Example 1

[0075] The difference between Comparative Example 1 and Example 1 is that the nano-activated calcium carbonate is replaced with ordinary heavy calcium carbonate (400 mesh) of equal mass, and the other conditions are the same as those of Example 1.

[0076] Test Example 1

[0077] The calcium hydrogen phosphate content, ignition loss, whiteness and application gas generation of the calcium hydrogen phosphate products prepared in Example 1 and Comparative Example 1 were tested, and the test method and test conditions were as follows:

[0078] The test method for calcium hydrogen phosphate content refers to GB 1886.3-2021;

[0079] The test method for loss on ignition refers to GB 1886.3-2021;

[0080] The whiteness of the product is tested using a WSB-3A whiteness meter;

[0081] Application gas production:

[0082] Bubble verification operation: (Requirement: no bubbles or a small amount of bubbles)

[0083] 1. Take 2g of citric acid monohydrate and add it to 100ml of room temperature purified water. Stir thoroughly until it is completely dissolved.

[0084] 2. Add 2g of calcium hydrogen phosphate, stir evenly, let stand for 1min, and observe the bubbles in the solution after shaking;

[0085] The test results are shown in Table 1.

[0086] Table 1

[0087] Sample No. Example 1 Comparative Example 1 Calcium hydrogen phosphate content (%) 101.01 98.76 Loss on ignition (%) 25.61 24.26 Product whiteness 98.5 85.2 Application Gas Production No bubbles generated A lot of bubbles are generated

[0088] It can be seen from the data in Table 1 that the use of ordinary heavy calcium carbonate to synthesize calcium hydrogen phosphate will reduce the whiteness of the calcium hydrogen phosphate product, and a large number of bubbles will appear during the application process. The calcium hydrogen phosphate prepared by the nano-activated calcium carbonate prepared in Example 1 of the present invention has high whiteness and no bubbles are generated during the application process, which can solve the problem of a large number of bubbles generated during the application of traditional calcium hydrogen phosphate.

[0089] (II) Effect of carbonization temperature (calcium carbonate particle size and whiteness) on the performance of final product calcium hydrogen phosphate:

[0090] Example 2

[0091] The difference between Example 2 and Example 1 is that the water bath heating temperature of the carbonization process in step S1 is 45° C., and the other conditions are the same as in Example 1.

[0092] Example 3

[0093] The difference between Example 3 and Example 1 is that the water bath heating temperature of the carbonization process in step S1 is 55° C., and the other conditions are the same as in Example 1.

[0094] Comparative Example 2

[0095] The difference between Comparative Example 2 and Example 1 is that the water bath heating temperature of the carbonization process in step S1 is 65° C., and the other conditions are the same as in Example 1.

[0096] Test Example 2

[0097] The particle size and whiteness of the nano-activated calcium carbonate prepared in Examples 1-3 and Comparative Example 2 were tested, and the calcium hydrogen phosphate content, ignition loss, whiteness and application gas generation of the final product calcium hydrogen phosphate were tested. The test method was the same as that of Test Example 1. The test results are shown in Table 2.

[0098] Table 2

[0099] Sample No. Example 1 Example 2 Example 3 Comparative Example 2 Carbonization temperature(℃) 35 45 55 65 Calcium carbonate particle size (nm) 54 98 110 250 Calcium carbonate whiteness 92.6 90.3 88.4 80.3 Calcium hydrogen phosphate content (%) 101.01 92.31 90.20 85.16 Dicalcium Phosphate Whiteness 98.5 90.1 82.7 73.2 Application Gas Production No bubbles Micro bubbles A small amount of bubbles Lots of bubbles

[0100] It can be seen from the data in Table 2 that different carbonization temperatures have a great influence on the particle size and whiteness of the generated calcium carbonate product. The higher the carbonization temperature, the larger the particle size of the generated calcium carbonate and the lower the whiteness, which leads to a decrease in the content and whiteness of the final product calcium hydrogen phosphate. When the particle size of calcium carbonate reaches 250nm, the generated calcium hydrogen phosphate will produce a large number of bubbles during application; when the particle size of calcium carbonate is reduced to 110nm, the prepared calcium hydrogen phosphate has a small amount of bubbles when used; when the particle size of calcium carbonate is reduced to 98nm, the prepared calcium hydrogen phosphate has only a small amount of bubbles when used, and when the particle size of calcium carbonate is reduced to 54nm, the prepared calcium hydrogen phosphate has no bubbles when used.

[0101] (III) Effect of crystal form regulator / crystal form on the performance of final product calcium hydrogen phosphate:

[0102] Example 4

[0103] The difference between Example 4 and Example 1 is that in step S1, the crystal form regulator is replaced with an equal amount of phosphoric acid to synthesize fibrous nano-activated calcium carbonate, and the other conditions are the same as in Example 1.

[0104] Comparative Example 3

[0105] The difference between Comparative Example 3 and Example 1 is that in step S1, no crystal form regulator is added, and the other conditions are the same as those in Example 1.

[0106] Test Example 3

[0107] The particle size of the calcium carbonate prepared in Example 1, Example 4 and Comparative Example 3 was tested, and the calcium hydrogen phosphate content and application gas production of the final product calcium hydrogen phosphate were tested. The testing method was the same as that of Test Example 1. The test results are shown in Table 3.

[0108] Table 3

[0109] Sample No. Example 1 Example 4 Comparative Example 3 Calcium carbonate particle size (nm) 54 160 3699 Calcium hydrogen phosphate content (%) 101.01 98.75 92.34 Application Gas Production No bubbles A small amount of bubbles Lots of bubbles

[0110] It can be seen from the data in Table 3 that the addition of a crystal form regulator can reduce the particle size of calcium carbonate, so that the reaction is more complete when preparing calcium hydrogen phosphate, the content of calcium hydrogen phosphate is higher, and the amount of bubbles generated during application is significantly reduced. Phosphoric acid is added as a crystal form regulator to generate fibrous calcium carbonate, which significantly reduces the particle size of calcium carbonate, increases the content of calcium hydrogen phosphate, and reduces the amount of bubbles generated when calcium hydrogen phosphate is used compared to the case where no crystal form regulator is added; compared to phosphoric acid, under the same process conditions, sulfuric acid is used as a crystal form regulator, and the generated cubic calcium carbonate has a smaller particle size, a larger specific surface area, a higher content of calcium hydrogen phosphate, and no bubbles are generated during its application.

[0111] (IV) Effect of surfactants on the performance of final product calcium hydrogen phosphate:

[0112] Example 5

[0113] The difference between Example 5 and Example 1 is that in step S2, the surfactant is replaced with an equal amount of 2-myristic acid monoglyceride, and the other conditions are the same as in Example 1.

[0114] Example 6

[0115] The difference between Example 6 and Example 1 is that in step S2, the surfactant is replaced with an equal amount of 11-octadecenoic acid, and the other conditions are the same as in Example 1.

[0116] Comparative Example 4

[0117] The difference between Comparative Example 4 and Example 1 is that in step S2, no surfactant is added, and the other conditions are the same as those in Example 1.

[0118] Test Example 4

[0119] The particle size of the calcium carbonate prepared in Example 1, Examples 5-6 and Comparative Example 4 was tested, and the calcium hydrogen phosphate content and application gas production of the final product calcium hydrogen phosphate were tested. The testing method was the same as that of Test Example 1. The test results are shown in Table 4.

[0120] Table 4

[0121] Sample No. Example 1 Example 5 Example 6 Comparative Example 4 Calcium carbonate primary particle size (nm) 54 60 80 58 Calcium carbonate secondary particle size (nm) / / / 360 Calcium hydrogen phosphate content (%) 101.01 98.56 91.20 90.12 Application Gas Production No bubbles No bubbles Micro bubbles Lots of bubbles

[0122] It can be seen from the data in Table 4 that calcium carbonate generated without adding a surfactant has a larger surface energy and a larger viscosity due to its fine particles, which is easy to produce secondary agglomeration and form particles with larger secondary particle size, so that it cannot fully react in the process of generating the final product calcium hydrogen phosphate, resulting in a decrease in the content of the final product calcium hydrogen phosphate, and a large number of bubbles will be generated in the product application. The use of 2-lauric acid glyceryl monoester, 2-myristic acid glyceryl monoester and C15-C18 fatty acid as surfactants can effectively avoid calcium carbonate agglomeration, reduce the particle size of calcium carbonate, and reduce the amount of bubbles generated when calcium hydrogen phosphate is used; under the same process conditions, the calcium carbonate prepared using 2-lauric acid glyceryl monoester and 2-myristic acid glyceryl monoester as surfactants has a smaller particle size, and the calcium hydrogen phosphate prepared under the optimal conditions can achieve the effect of no bubble generation when used.

[0123] (V) Effect of calcium carbonate moisture on the performance of the final product calcium hydrogen phosphate:

[0124] Example 7

[0125] The difference between Example 7 and Example 1 is that in step S2, the drying temperature is 180°C, and the other conditions are the same as in Example 1.

[0126] Example 8

[0127] The difference between Example 8 and Example 1 is that in step S2, the drying temperature is 150°C, and the other conditions are the same as Example 1.

[0128] Comparative Example 5

[0129] The difference between Comparative Example 5 and Example 1 is that in step S2, the drying temperature is 100°C, and the other conditions are the same as Example 1.

[0130] Test Example 5

[0131] The moisture content of the calcium carbonate prepared in Example 1, Examples 7-8 and Comparative Example 5 was tested, and the calcium hydrogen phosphate content and application gas production of the final product calcium hydrogen phosphate were tested. The testing method was the same as that of Test Example 1. The test results are shown in Table 5.

[0132] Table 5

[0133] Sample No. Example 1 Example 7 Example 8 Comparative Example 5 Drying temperature (℃) 200 180 150 100 Calcium carbonate moisture (wt%) 0.15 2.36 5.69 12.10 Calcium hydrogen phosphate content (%) 101.01 96.15 95.86 93.57 Application Gas Production No bubbles Micro bubbles A small amount of bubbles Lots of bubbles

[0134] It can be seen from the data in Table 5 that different drying conditions have a great influence on the moisture content of calcium carbonate products. The production of calcium carbonate with higher moisture content will reduce the degree of reaction in the process of preparing the final product calcium hydrogen phosphate, thereby causing the content of calcium hydrogen phosphate in the final product to decrease. Bubbles will be generated in the final product during its application. Therefore, in the process of synthesizing calcium carbonate, it is necessary to reasonably control the drying conditions to control the moisture content of calcium carbonate.

[0135] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.

Claims

1. A method for preparing calcium hydrogen phosphate, characterized in that: The following steps are involved: Nano-active calcium carbonate is used as a calcium source to react with phosphoric acid to produce calcium hydrogen phosphate; The nanometer active calcium carbonate has a cubic crystal form and / or a fibrous form, a particle size of 30-200 nm, a moisture content of less than 6%, and a whiteness of more than 88%.

2. The method for preparing calcium hydrogen phosphate according to claim 1, wherein The nano active calcium carbonate has a cubic crystal form, a particle size of 30-100 nm, a moisture content of less than 2.5%, and a whiteness of ≥90.

3. The method for preparing calcium hydrogen phosphate according to claim 1, characterized in that The preparation method of the nano active calcium carbonate comprises the following steps: S1. CO2 gas is introduced into the calcium hydroxide suspension, and a crystal modifier is added to perform a carbonization reaction to obtain a calcium carbonate slurry; S2. Add a surfactant to the calcium carbonate slurry for stirring and activation, solid-liquid separation, washing, and drying to obtain the nano-activated calcium carbonate.

4. The method for preparing calcium hydrogen phosphate according to claim 3, characterized in that: Step S1 includes at least one of the following features (1)-(4): (1) The mass concentration of the calcium hydroxide suspension is 20%-30%; (2) The temperature of the carbonization reaction is 30-60°C; (3) the carbonization reaction step comprises: firstly introducing CO2 gas to carbonize the slurry until the pH value of the slurry is 7-8, then adding the crystal form regulator, and then continuing to introduce CO2 gas to carbonize the slurry until the pH value of the slurry is 5-6, thereby obtaining the calcium carbonate slurry; (4) The crystal form regulator includes sulfuric acid and / or phosphoric acid.

5. The method for preparing calcium hydrogen phosphate according to claim 3, characterized in that: In step S2, at least one of the following features (1) to (4) is included: (1) The surfactant includes at least one of 2-lauric acid glyceryl monoester, 2-myristic acid glyceryl monoester, and C15-C18 fatty acid; (2) The amount of the surfactant is 5%-10% by weight of calcium carbonate; (3) The stirring activation temperature is 70-90° C., and the stirring activation time is 0.5-3.5 h; (4) The drying temperature is 150-230°C, and the drying time is 16-20 hours.

6. The method for preparing calcium hydrogen phosphate according to claim 1, characterized in that: The preparation method of described calcium hydrogen phosphate comprises the following steps: The nano-active calcium carbonate is dispersed in water to prepare a calcium carbonate suspension; the calcium carbonate suspension is added dropwise to a phosphoric acid solution, the pH is adjusted to 2.5-3.5, and the solution is fully reacted; the pH is adjusted to 4-5 with a calcium hydroxide solution, and after the solution is fully reacted, the solution is aged, solid-liquid separated, and dried to obtain the calcium hydrogen phosphate.

7. The method for preparing calcium hydrogen phosphate according to claim 6, characterized in that: The synthesis temperature of the calcium hydrogen phosphate is 30-50° C., and the reaction time is: the calcium carbonate suspension is added dropwise to the phosphoric acid solution and reacted for 1-2 hours, and the pH is adjusted with the calcium hydroxide solution and reacted for 1-2 hours.

8. The method for preparing calcium hydrogen phosphate according to claim 6, characterized in that: The mass concentration of the phosphoric acid solution is 35%-60%.

9. The method for preparing calcium hydrogen phosphate according to claim 6, characterized in that: The dropping speed of the calcium carbonate suspension is 5-10 mL / min, and the molar ratio of the nano-active calcium carbonate to the phosphoric acid is 1:1.5-1.

7.

10. A calcium hydrogen phosphate, characterized in that: The calcium hydrogen phosphate is prepared by the preparation method of calcium hydrogen phosphate according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for manufacturing nano calcium carbonate from high-concentration carbon dioxide industrial exhaust gases

    CN101723429A

  • Production method of superfine calcium hydrophosphate

    CN111268661A

  • Process for producing calcium hydrogen phosphate dihydrate and fluorine insolubilizer

    WO2011064836A1