Nitrogen and sulfur co-doped functionalized durian shell-derived hard carbon material as well as preparation method and application thereof
Through nitrogen-sulfur co-doping functional modification, the problems of poor conductivity and low capacity of biomass-derived hard carbon materials in sodium-ion battery applications have been solved, and their Coulombic efficiency and rate performance have been significantly improved, achieving efficient sodium Properties of negative electrode materials for ion batteries.
Patent Information
- Application Number
- CN202410911283.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-29
AI Technical Summary
Existing biomass-derived hard carbon materials have problems with poor conductivity, low first Coulombic efficiency, and low reversible capacity in sodium-ion battery applications, making it difficult to meet commercial application requirements.
Using the nitrogen-sulfur co-doping functional modification method, a nitrogen-sulfur co-doping functionalized durian shell-derived hard carbon material was prepared through pretreatment, hydrothermal pickling, hydrothermal doping and high-temperature carbonization steps to improve its performance. Structural compactness and battery capacity.
Significantly improve the conductivity and reactivity of hard carbon materials, achieve high Coulombic efficiency and specific capacity, enhance the rate performance of sodium-ion battery anode materials, the first discharge capacity reaches 246.1mAh/g, the first efficiency exceeds 86%, and in The discharge capacity is still 60.1mAh/g at 5C high current density.
Smart Images

Figure CN118851150A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrochemical energy storage, and in particular to a nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material, and a preparation method and application thereof. Background Art
[0002] Energy storage is one of the important supporting technologies for achieving the goals of carbon peak and carbon neutrality. It is also an important means to smooth out the fluctuations of new energy and reduce the impact of large-scale new energy access on the power grid. At present, global competition for energy resources is becoming increasingly fierce, and my country is also facing major changes in the adjustment of its energy structure. The proportion of electrochemical energy storage in the energy structure has increased year by year, and electrochemical energy storage is currently dominated by lithium batteries and lead-acid batteries. Among them, lead-acid batteries will gradually be eliminated by the market due to their low energy density, short cycle life and great harm from lead pollution. Lithium-ion batteries are widely used in actual production and life because of their high energy density, high open circuit voltage, high output power and no memory effect. However, lithium resources in the earth's crust are scarce and unevenly distributed, making it difficult to meet the growing market demand. Based on this, sodium-ion batteries have emerged in the field of energy storage as a new type of battery technology with their cost advantages and resource advantages.
[0003] Negative electrode materials with high specific capacity, low cost, environmental friendliness and good stability are the key to realizing the application of high-performance sodium-ion batteries in energy storage systems. Among them, hard carbon exhibits excellent sodium storage performance due to its structural advantages such as large interlayer spacing, many nanopores, and rich defect sites. In addition, in recent years, with the realization of the "dual carbon" goals, the reuse of waste biomass is crucial to reducing resource consumption, improving resource utilization efficiency, and achieving synergistic efficiency of pollution reduction and carbon reduction. Therefore, combined with the current application needs of sodium-ion battery energy storage, it is of great significance to realize the efficient resource utilization of waste biomass and convert it into high-value-added biomass-derived hard carbon energy storage materials.
[0004] Biomass-derived carbon materials have attracted extensive attention from researchers at home and abroad due to their wide raw material sources, renewable nature, and low price. For example, some researchers have prepared hard carbon materials using waste biomass such as coconut shells and rice husks as raw materials and used them as negative electrode materials for sodium ion batteries, achieving good sodium storage performance. ([1] Sui Mengjia, An Yuliang, Ren Yujie, et al. Research on the preparation of rice husk-based silicon-carbon lithium ion battery negative electrode materials [J]. Chemistry and Adhesion, 2023, 45(04): 289-299.) Against the above background, a Chinese patent (ZL202211276795.X) discloses a durian shell-based hard carbon negative electrode material and a preparation method thereof, wherein the durian shell powder is pretreated by acid immersion, pre-carbonized in an inert atmosphere, alkali leached and then acid leached, and carbonized in an inert atmosphere to obtain a durian shell-based hard carbon negative electrode material. Although hard carbon anode materials prepared from biomass as raw materials have the characteristics of wide sources, low cost, simple preparation and environmental friendliness, they still face the common disadvantages of hard carbon materials, such as poor conductivity, low first coulombic efficiency and low reversible capacity. Therefore, it is crucial to optimize the preparation method of biomass-derived hard carbon materials and perform functional modification to improve their sodium storage performance to meet the requirements of commercial applications. Summary of the invention
[0005] In order to solve the above problems, the purpose of the present invention is to provide a nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material and its preparation method and application. Discarded durian shell is used as raw material, and the nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material is obtained through pretreatment, hydrothermal pickling, hydrothermal doping, and high-temperature carbonization. In the preparation method, hydrothermal pickling enables more thorough removal of impurities, and the structure of the prepared hard carbon material is more compact. The compaction density of the obtained hard carbon material is large, which can effectively improve the battery capacity. In addition, the present invention uses ammonium sulfide solution as a nitrogen and sulfur source to dope nitrogen and sulfur elements. The doping of nitrogen and sulfur elements is the main factor in functional modification. From the experimental data, the performance of the negative electrode material after doping is better. The use of peel biomass waste to prepare carbon negative electrode materials not only saves costs, but also solves the environmental pollution caused by peel waste. The present invention obtains a sodium ion battery negative electrode material with high coulombic efficiency, specific capacity and rate performance through a nitrogen-sulfur doped modified biomass-derived hard carbon strategy.
[0006] In order to achieve the above object, the present invention discloses a method for preparing a nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material, comprising the following steps:
[0007] (1) Pretreatment: drying and crushing the durian shell to millimeter level to obtain durian shell solid particles;
[0008] (2) hydrothermal pickling: placing the durian shell solid particles obtained in step (1) in a hydrothermal kettle A, adding an acid solution into the hydrothermal kettle A, and then placing the hydrothermal kettle A in a forced air drying oven for hydrothermal pickling treatment, followed by cooling to room temperature, filtering the obtained product, washing with water until neutral, and then drying to obtain a durian shell-derived carbon precursor;
[0009] (3) Hydrothermal doping: placing the carbon precursor derived from durian shell obtained in step (2) in a hydrothermal reactor B, adding an aqueous solution of ammonium sulfide, placing the hydrothermal reactor B in a forced air drying oven for hydrothermal doping treatment, then cooling to room temperature, filtering and drying the obtained product to obtain a doped and modified carbon precursor intermediate;
[0010] (4) High temperature carbonization: placing the doped and modified carbon precursor intermediate obtained in step (3) in a tube furnace and subjecting it to high temperature carbonization treatment in an inert atmosphere, cooling it naturally to room temperature, and finely grinding the obtained product to obtain a nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material.
[0011] Preferably, the drying in step (1) is forced air drying, the forced air drying temperature is 50-100°C, and the drying time is 12-36h; the pulverizing is performed by a wall breaker, the wall breaker has a power of 900-3000W, and a rotation speed of 20000-45000r / min. After crushing, the powder particle size is between 0.1 and 0.4mm, that is, it can pass through a 40-150 mesh sieve.
[0012] Preferably, the acid in the acid solution in step (2) includes but is not limited to one of sulfuric acid, hydrochloric acid, and phosphoric acid, and the concentration of the acid solution is 0.01 to 1.0 mol / L;
[0013] Preferably, after the acid solution is added to the hydrothermal kettle A in step (2), the filling rate of the hydrothermal kettle A is 50%-90%, the reaction temperature of the hydrothermal pickling treatment is 100-180° C., and the reaction time is 2-8 hours.
[0014] Preferably, in step (2), the mass ratio of the durian shell solid particles to the acid solution is 1:4-20.
[0015] Preferably, the concentration of the aqueous ammonium sulfide solution in step (3) is 0.01 to 1.0 mol / L.
[0016] Preferably, after the ammonium sulfide aqueous solution is added to the hydrothermal kettle B in step (3), the filling rate of the hydrothermal kettle B is 50%-90%; the reaction time of the hydrothermal doping treatment is 2-8h, and the reaction temperature is 180-250°C.
[0017] Preferably, the mass ratio of the carbon precursor derived from durian shell to the aqueous ammonium sulfide solution in step (3) is 1:5-20.
[0018] Preferably, the inert atmosphere in step (4) is one of argon or nitrogen, and the inert atmosphere flow rate is 100 to 200 sccm; the high-temperature carbonization treatment is specifically to raise the temperature of the tubular furnace from room temperature to 800 to 1200°C, and keep it warm for 2 to 4 hours, with a heating rate of 5°C / min, and naturally cool to room temperature after the insulation is completed.
[0019] Preferably, the fine grinding in step (4) is to dry-mill the obtained product in a ball mill and grind it to the micron level, and after fine grinding, the obtained powder is passed through a 500-mesh sieve to obtain a nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material.
[0020] Preferably, in step (4), the obtained product is placed in an agate jar for dry ball milling, and the mass ratio of agate balls to the obtained product is maintained at 20:1.
[0021] Preferably, in step (4), the ball mill is operated at 200-400 rpm for 3-6 hours, and the rotation direction is reversed every 60 minutes.
[0022] The present invention also discloses a nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material prepared according to the method and application of the nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material as a negative electrode material for a sodium ion battery.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) The preparation method provided by the present invention is simple, efficient and low-cost. The waste biomass durian shell is used, and the selected material is renewable, widely available and low-priced. By using simple and efficient element doping modification, combined with hydrothermal pickling and secondary hydrothermal doping steps, effective impurity removal and functional modification of hard carbon materials can be achieved; in addition, no harmful substances are produced during the synthesis process, which is in line with the concept of green chemistry;
[0025] (2) The nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material prepared by the method of the present invention has a change in material structure and an increase in surface wrinkles due to the introduction of N and S elements. The surface area of the material is increased without changing its overall flaky morphology, providing abundant active sites, which is beneficial to improving the sodium storage performance of the hard carbon material. In addition, the doped hard carbon material also has good conductivity and reaction activity. The nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material is used as a negative electrode material for sodium ion batteries, which has good capacity and rate performance. At a current density of 0.1C, the first discharge capacity of the hard carbon material is as high as 246.1mAh / g, and the first efficiency exceeds 86%. Even at a high current density of 5C, the discharge capacity is still 60.1mAh / g. Raman testing confirms that the I D / IG The value decreased from 1.04 to 0.97, which also proves that the material has good conductivity and reactivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The scanning electron microscope morphology image and EDS image of the nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material prepared in Example 1, wherein the images marked as (a) and (b) in the upper left corner are scanning electron microscope morphology images, and the images below images (a) and (b) are both images (c), and image (c) is an EDS image;
[0027] Figure 2 The XRD diffraction pattern of the nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material prepared in Example 1;
[0028] Figure 3 Raman characterization images of the nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material prepared in Example 1, the nitrogen-doped durian shell-derived hard carbon material prepared in Comparative Example 1, the pure durian shell-derived hard carbon material prepared in Comparative Example 2 after hydrothermal pickling and high-temperature carbonization, and the pure durian shell-derived hard carbon material prepared in Comparative Example 3 after no pickling and only high-temperature carbonization;
[0029] Figure 4 The scanning electron microscope morphology images and EDS images of the nitrogen-doped durian shell-derived hard carbon material prepared in Comparative Example 1, wherein the images marked as (a) and (b) in the upper left corner are scanning electron microscope morphology images, and the images below (a) and (b) are both images (c), and image (c) is an EDS image;
[0030] Figure 5 The XRD diffraction pattern of the nitrogen-doped durian shell-derived hard carbon material prepared in Comparative Example 1;
[0031] Figure 6 The scanning electron microscope morphology image and EDS image of the hard carbon material derived from pure durian shell obtained after hydrothermal pickling and high-temperature carbonization prepared in Comparative Example 2, wherein the images marked as (a) and (b) in the upper left corner are scanning electron microscope morphology images, and the images below images (a) and (b) are all images (c), and image (c) is an EDS image;
[0032] Figure 7 The XRD diffraction pattern of the hard carbon material derived from pure durian shell obtained after hydrothermal pickling and high-temperature carbonization prepared in Comparative Example 2;
[0033] Figure 8The scanning electron microscope morphology and EDS spectrum of the hard carbon material derived from pure durian shell obtained by high-temperature carbonization without acid washing prepared in Comparative Example 3, wherein the upper left corners marked as (a) and (b) are scanning electron microscope morphology images, and the images below (a) and (b) are all (c), and (c) is an EDS image;
[0034] Fig. 9 The XRD diffraction pattern of the hard carbon material derived from pure durian shell obtained by high temperature carbonization without acid washing prepared in Comparative Example 3;
[0035] Fig.10 This is a rate performance test diagram of the nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material prepared in Example 1 as a negative electrode material for a sodium ion battery;
[0036] Fig.11 This is a rate performance test diagram of the nitrogen-doped durian shell-derived hard carbon material prepared in Comparative Example 1 as a negative electrode material for a sodium ion battery;
[0037] Fig.12 This is a rate performance diagram of the hard carbon material derived from pure durian shell obtained after hydrothermal pickling and high-temperature carbonization prepared in Comparative Example 2 as a negative electrode material for a sodium ion battery;
[0038] Fig.13 This is a rate performance diagram of the hard carbon material derived from pure durian shell obtained by high-temperature carbonization without acid washing prepared in Comparative Example 3 as a negative electrode material for sodium ion batteries. DETAILED DESCRIPTION
[0039] In order to better understand the content of the present invention, the present invention will be further described below in conjunction with specific embodiments and drawings. The following embodiments are implemented based on the technology of the present invention, and detailed implementation methods and operating steps are given, but the protection scope of the present invention is not limited to the following embodiments.
[0040] Embodiment 1:
[0041] (1) Pretreatment: 100 g of clean discarded durian shells were placed in a blast drying oven and dried at 100° C. After drying for 12 h, they were crushed in a wall-breaking machine with a power of 2500 W and a rotation speed of 32000 r / min for 5 min to preliminarily obtain dry and crushed durian shell solid particles (denoted as DP) with a particle size between 0.1 and 0.3 mm;
[0042] (2) Hydrothermal acid washing: 5 g of the durian shell solid particles (DP) obtained in step (1) were placed in a 100 mL hydrothermal kettle, and 70 mL of a 0.1 mol / L dilute hydrochloric acid solution was added. The filling rate of the hydrothermal kettle was about 70%, and then the hydrothermal kettle was placed in a forced air drying oven for hydrothermal acid washing. Specifically, the reaction was carried out at 120° C. for 6 h. After the reaction was completed, the mixture was cooled to room temperature, and the obtained product was filtered, washed with water until neutral, and then dried to obtain a durian shell-derived carbon precursor (denoted as H-DP);
[0043] (3) Hydrothermal doping: 5 g of the durian shell-derived carbon precursor (H-DP) obtained in step (2) was placed in another 100 mL hydrothermal kettle, and 70 mL of 0.2 mol / L ammonium sulfide aqueous solution was added. The filling rate of the hydrothermal kettle reached 70%. The hydrothermal kettle was placed in a forced air drying oven for hydrothermal doping treatment. Specifically, the reaction was carried out at 200° C. for 6 h. After the reaction was completed, the reaction was cooled to room temperature. The obtained product was filtered and dried at 100° C. to obtain a doped and modified carbon precursor intermediate (denoted as NS-HDP);
[0044] (4) High temperature carbonization: 2 g of the doped and modified carbon precursor intermediate (NS-HDP) obtained in step (3) was placed in a tube furnace and subjected to high temperature carbonization treatment in an inert atmosphere. Specifically, the NS-HDP was placed in a porcelain boat and the porcelain boat was placed in the middle of the tube furnace. The temperature was raised to 1000°C at a heating rate of 5°C / min under a pure nitrogen atmosphere of 100 sccm, and the temperature was kept for 2 hours. After the temperature was kept, the mixture was naturally cooled to room temperature. The obtained product was finely ground, specifically, the obtained product was placed in an agate jar, and the agate jar was placed in a ball mill for dry ball milling. The mass ratio of the agate balls used to the sample material was maintained at 20:1. The ball mill was operated at 200 rpm for 4 hours, and the rotation direction was reversed every 60 minutes. The powder obtained after fine grinding was passed through a 500-mesh sieve to obtain the final nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material (denoted as NS-DS).
[0045] Embodiment 2:
[0046] (1) Pretreatment: 100 g of clean discarded durian shells were placed in a blast drying oven and dried at 100° C. After drying for 12 h, they were crushed in a wall-breaking machine with a power of 2500 W and a rotation speed of 32000 r / min for 5 min to preliminarily obtain dry and crushed durian shell solid particles (denoted as DP) with a particle size between 0.1 and 0.3 mm;
[0047] (2) Hydrothermal pickling: 5 g of the durian shell solid particles (DP) obtained in step (1) were placed in a 100 mL hydrothermal kettle, and 70 mL of a 0.25 mol / L dilute hydrochloric acid solution was added. The filling rate of the hydrothermal kettle was about 70%, and then the hydrothermal kettle was placed in a forced air drying oven for hydrothermal pickling treatment. Specifically, the reaction was carried out at 150° C. for 4 h. After the reaction was completed, the mixture was cooled to room temperature, and the obtained product was filtered, washed with water until neutral, and then dried to obtain a durian shell-derived carbon precursor (denoted as H-DP);
[0048] (3) Hydrothermal doping: 5 g of the durian shell-derived carbon precursor (H-DP) obtained in step (2) was placed in another 100 mL hydrothermal kettle, and 70 mL of 0.5 mol / L ammonium sulfide aqueous solution was added. The filling rate of the hydrothermal kettle was about 70%. The hydrothermal kettle was placed in a forced air drying oven for hydrothermal doping treatment. Specifically, the reaction was carried out at 180° C. for 6 h. After the reaction was completed, the reaction was cooled to room temperature. The obtained product was filtered and dried at 100° C. to obtain a doped and modified carbon precursor intermediate (denoted as NS-HDP);
[0049] (4) High temperature carbonization: 2 g of the doped and modified carbon precursor intermediate (NS-HDP) obtained in step (3) was placed in a tube furnace and subjected to high temperature carbonization treatment in an inert atmosphere. Specifically, the NS-HDP was placed in a porcelain boat and the porcelain boat was placed in the middle of the tube furnace. The temperature was raised to 900°C at a heating rate of 5°C / min under a pure nitrogen atmosphere of 100 sccm, and the temperature was kept for 2 hours. After the temperature was kept, the mixture was naturally cooled to room temperature. The obtained product was finely ground, specifically, the obtained product was placed in an agate jar, and the agate jar was placed in a ball mill for dry ball milling. The mass ratio of the agate balls used to the sample material was maintained at 20:1. The ball mill was operated at 200 rpm for 4 hours, and the rotation direction was reversed every 60 minutes. The powder obtained after fine grinding was passed through a 500-mesh sieve to obtain the final nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material (denoted as NS-DS).
[0050] Embodiment 3:
[0051] (1) Pretreatment: 100 g of clean discarded durian shells were placed in a blast drying oven and dried at 100° C. After drying for 12 h, they were crushed in a wall-breaking machine with a power of 2500 W and a rotation speed of 32000 r / min for 5 min to preliminarily obtain dry and crushed durian shell solid particles (denoted as DP) with a particle size between 0.1 and 0.3 mm;
[0052] (2) Hydrothermal pickling: 5 g of the durian shell solid particles (DP) obtained in step (1) were placed in a 100 mL hydrothermal kettle, and 70 mL of a 0.5 mol / L dilute hydrochloric acid solution was added. The filling rate of the hydrothermal kettle was about 70%, and then the hydrothermal kettle was placed in a forced air drying oven for hydrothermal pickling treatment. Specifically, the reaction was carried out at 180° C. for 3 h. After the reaction was completed, the mixture was cooled to room temperature, and the obtained product was filtered, washed with water until neutral, and then dried to obtain a durian shell-derived carbon precursor (denoted as H-DP);
[0053] (3) Hydrothermal doping: 5 g of the durian shell-derived carbon precursor (H-DP) obtained in step (2) was placed in another 100 mL hydrothermal kettle, and 70 mL of 0.1 mol / L ammonium sulfide aqueous solution was added. The filling rate of the hydrothermal kettle was about 70%. The hydrothermal kettle was placed in a forced air drying oven for hydrothermal doping treatment. Specifically, the reaction was carried out at 220° C. for 3 h. After the reaction was completed, the reaction was cooled to room temperature. The obtained product was filtered and dried at 100° C. to obtain a doped and modified carbon precursor intermediate (denoted as NS-HDP);
[0054] (4) High temperature carbonization: 2 g of the doped and modified carbon precursor intermediate (NS-HDP) obtained in step (3) was placed in a tube furnace and subjected to high temperature carbonization treatment in an inert atmosphere. Specifically, the NS-HDP was placed in a porcelain boat and the porcelain boat was placed in the middle of the tube furnace. The temperature was raised to 1100°C at a heating rate of 5°C / min under a pure nitrogen atmosphere of 100 sccm, and the temperature was kept for 2 hours. After the temperature was kept, the mixture was naturally cooled to room temperature. The obtained product was finely ground, specifically, the obtained product was placed in an agate jar, and the agate jar was placed in a ball mill for dry ball milling. The mass ratio of the agate balls used to the sample material was maintained at 20:1. The ball mill was operated at 200 rpm for 4 hours, and the rotation direction was reversed every 60 minutes. The powder obtained after fine grinding was passed through a 500-mesh sieve to obtain the final nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material (denoted as NS-DS).
[0055] Comparative Example 1:
[0056] (1) Pretreatment: 100 g of clean discarded durian shells were placed in a blast drying oven and dried at 100° C. After drying for 12 h, they were crushed in a wall-breaking machine with a power of 2500 W and a rotation speed of 32000 r / min for 5 min to preliminarily obtain dry and crushed durian shell solid particles (denoted as DP) with a particle size between 0.1 and 0.3 mm;
[0057] (2) Hydrothermal acid washing: 5 g of the durian shell solid particles (DP) obtained in step (1) were placed in a 100 mL hydrothermal kettle, and 70 mL of a 0.1 mol / L dilute hydrochloric acid solution was added. The filling rate of the hydrothermal kettle was about 70%, and then the hydrothermal kettle was placed in a forced air drying oven for hydrothermal acid washing. Specifically, the reaction was carried out at 120° C. for 6 h. After the reaction was completed, the mixture was cooled to room temperature, and the obtained product was filtered, washed with water until neutral, and then dried to obtain a durian shell-derived carbon precursor (denoted as H-DP);
[0058] (3) Hydrothermal doping: 5 g of the carbon precursor (H-DP) derived from the durian shell obtained in step (2) was placed in another 100 mL hydrothermal kettle, and 70 mL of a 0.2 mol / L dinitrile amide aqueous solution was added. The filling rate of the hydrothermal kettle was about 70%. The hydrothermal kettle was placed in a forced air drying oven for hydrothermal doping treatment. Specifically, the reaction was carried out at 200° C. for 6 h. After the reaction was completed, the reaction was cooled to room temperature. The obtained product was filtered and dried at 100° C. to obtain a nitrogen-doped intermediate (denoted as N-HDP);
[0059] (4) High temperature carbonization: 2 g of the doped and modified intermediate (N-HDP) obtained in step (3) was placed in a tube furnace and subjected to high temperature carbonization treatment in an inert atmosphere. Specifically, the N-HDP was placed in a porcelain boat and the porcelain boat was placed in the middle of the tube furnace. The temperature was raised to 1000°C at a heating rate of 5°C / min under a pure nitrogen atmosphere of 100 sccm, and the temperature was kept for 2 hours. After the temperature was kept, the mixture was naturally cooled to room temperature. The obtained product was finely ground, specifically, the obtained product was placed in an agate jar, and the agate jar was placed in a ball mill for dry ball milling. The mass ratio of the agate balls used to the sample material was maintained at 20:1. The ball mill was operated at 200 rpm for 4 hours, and the rotation direction was reversed every 60 minutes. The powder obtained after fine grinding was passed through a 500-mesh sieve to obtain a nitrogen-doped durian shell-derived hard carbon material (denoted as N-DS).
[0060] Comparative Example 2:
[0061] (1) Pretreatment: 100 g of clean discarded durian shells were placed in a blast drying oven and dried at 100° C. After drying for 12 h, they were crushed in a wall-breaking machine with a power of 2500 W and a rotation speed of 32000 r / min for 5 min to preliminarily obtain dry and crushed durian shell solid particles (denoted as DP) with a particle size between 0.1 and 0.3 mm;
[0062] (2) Hydrothermal acid washing: 5 g of the durian shell solid particles (DP) obtained in step (1) were placed in a 100 mL hydrothermal kettle, and 70 mL of a 0.1 mol / L dilute hydrochloric acid solution was added. The filling rate of the hydrothermal kettle was about 70%, and then the hydrothermal kettle was placed in a forced air drying oven for hydrothermal acid washing. Specifically, the reaction was carried out at 120° C. for 6 h. After the reaction was completed, the mixture was cooled to room temperature, and the obtained product was filtered, washed with water until neutral, and then dried to obtain a durian shell-derived carbon precursor (denoted as H-DP);
[0063] (3) High temperature carbonization: 2 g of the carbon precursor derived from durian shell (H-DP) obtained in step (2) was placed in a tube furnace and subjected to high temperature carbonization treatment in an inert atmosphere. Specifically, the carbon precursor derived from durian shell was placed in a porcelain boat and the porcelain boat was placed in the middle of the tube furnace. The temperature was raised to 1000°C at a heating rate of 5°C / min under a pure nitrogen atmosphere of 100 sccm, and the temperature was kept for 2 hours. After the temperature was kept, it was naturally cooled to room temperature. The obtained product was finely ground, specifically, the obtained product was placed in an agate jar, and the agate jar was placed in a ball mill for dry ball milling. The mass ratio of the agate balls used to the sample material was maintained at 20:1. The ball mill was operated at 200 rpm for 4 hours, and the rotation direction was reversed every 60 minutes. The powder obtained after fine grinding was passed through a 500 mesh sieve to obtain a pure durian shell-derived hard carbon material (referred to as H-DS) after hydrothermal pickling and high temperature carbonization.
[0064] Comparative Example 3:
[0065] (1) Pretreatment: 100 g of clean discarded durian shells were placed in a blast drying oven and dried at 100° C. After drying for 12 h, they were crushed in a wall-breaking machine with a power of 2500 W and a rotation speed of 32000 r / min for 5 min to preliminarily obtain dry and crushed durian shell solid particles (denoted as DP) with a particle size between 0.1 and 0.3 mm;
[0066] (2) High temperature carbonization: 2 g of the durian shell solid particles (DP) obtained in step (1) were placed in a tube furnace and subjected to high temperature carbonization treatment in an inert atmosphere. Specifically, the carbon precursor derived from the durian shell was placed in a porcelain boat and the porcelain boat was placed in the middle of the tube furnace. The temperature was raised to 1000°C at a heating rate of 5°C / min under a pure nitrogen atmosphere of 100 sccm, and the temperature was kept for 2 hours. After the temperature was kept, it was naturally cooled to room temperature. The obtained product was finely ground, specifically, the obtained product was placed in an agate jar, and the agate jar was placed in a ball mill for dry ball milling. The mass ratio of the agate balls used to the sample material was maintained at 20:1. The ball mill was operated at 200 rpm for 4 hours, and the rotation direction was reversed every 60 minutes. The powder obtained after fine grinding was passed through a 500 mesh sieve to obtain a pure durian shell-derived hard carbon material (denoted as DS) that was not acid-washed and only high-temperature carbonized.
[0067] Figure 1 The scanning electron microscope morphology image and EDS image of the nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material (NS-DS) prepared in Example 1, wherein the upper left corners are marked as (a) and (b) are scanning electron microscope morphology images, and the images located below (a) and (b) are all Figure (c), and Figure (c) is an EDS image. Figures (a) and (b) show the surface and cross-sectional scanning electron microscope morphology images of NS-DS. It can be seen that the doping of N and S elements causes changes in the material structure, and the surface wrinkles are more obvious. The thickness of the sheet is about 0.38μm, which increases the surface area of the material without changing its overall sheet morphology structure. It can be clearly observed from the EDS element distribution diagram in Figure (c) that the N and S elements are successfully doped and evenly distributed.
[0068] Figure 2 The XRD diffraction pattern of the nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material (NS-DS) prepared in Example 1 shows that the XRD of NS-DS has strong diffraction peaks at 2θ=23.25° and 43.69°, corresponding to the (002) and (101) crystal planes of the hard carbon material (standard card PDF#75-1621), and no other impurity peaks, indicating that a high-purity hard carbon material has been successfully prepared. The left shift of its carbon characteristic peak is due to the increase in the lattice constant caused by the doping of heteroatoms, which indirectly indicates that the N and S elements have been successfully introduced. The doped hard carbon material has good conductivity and reactivity, which is beneficial to improving its sodium storage performance.
[0069] Figure 3 The Raman comparison characterization diagrams are of the nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material (NS-DS) prepared in Example 1, the nitrogen-doped durian shell-derived hard carbon material (N-DS) prepared in Comparative Example 1, the pure durian shell-derived hard carbon material (H-DS) prepared in Comparative Example 2 after hydrothermal pickling and high-temperature carbonization, and the pure durian shell-derived hard carbon material (DS) prepared in Comparative Example 3 after no pickling and only high-temperature carbonization. It can be seen that at 1349 cm -1 (D band) and 1586cm -1 (G band) has two obvious peaks, through I D / I G The defect structure and graphitization degree of the prepared carbon material can be effectively judged. D / I G The value is 0.94, which indicates that it has a higher degree of graphitization and a lower degree of defect. D / I GThe value increased to 1.04, indicating that after the impurities were removed by pickling, the defects in the material increased significantly and the conductivity decreased. The I D / I G The values are 0.98 and 0.97 respectively. Compared with the pure durian shell derived hard carbon material (H-DS) treated with hydrochloric acid, the defects are relatively reduced. The introduction of heteroatoms changes the material structure, reduces its defects and improves its conductivity. The I of the nitrogen-sulfur co-doped durian shell derived hard carbon material (NS-DS) is higher than that of the nitrogen-doped durian shell derived hard carbon material (N-DS). D / I G The slightly smaller value may be due to the synergistic effect of N and S, which slightly increases the degree of graphitization, thereby improving the conductivity and reactivity of the material.
[0070] Figure 4 The scanning electron microscope morphology and EDS images of the nitrogen-doped durian shell-derived hard carbon material (N-DS) prepared in Comparative Example 1, where the upper left corners marked as (a) and (b) are scanning electron microscope morphology images, and the images below (a) and (b) are all Figure (c), and Figure (c) is an EDS image; Figures (a) and (b) show the scanning electron microscope morphology images of N-DS at different magnification scales. It can be seen from the figure that the N element is successfully introduced on the flaky carbon substrate and causes subtle changes in the structure, generating wrinkles on its surface, increasing the surface area of the material, enabling it to expose more active sites and improve its electrochemical performance. It can be clearly seen from the EDS distribution diagram of Figure (c) that the N element is successfully doped and evenly distributed.
[0071] Figure 5 The XRD diffraction pattern of the nitrogen-doped durian shell-derived hard carbon material (N-DS) prepared in Comparative Example 1 shows that the XRD of N-DS has strong diffraction peaks at 2θ=23.27° and 43.45°, corresponding to the (002) and (101) crystal planes of the hard carbon material (standard card PDF#75-1621), and no other impurity peaks, indicating that a high-purity hard carbon material has been successfully prepared. The left shift of its carbon characteristic peak is due to the increase in the lattice constant caused by the doping of heteroatoms, which indirectly indicates that the N element has been successfully introduced. The introduction of the N element increases the crystal defects of the carbon matrix material. The doped hard carbon material has good conductivity and reactivity, which is beneficial to improving its sodium storage performance.
[0072] Figure 6The scanning electron microscope morphology and EDS spectrum of the hard carbon material (H-DS) derived from pure durian shell obtained after hydrothermal pickling and high-temperature carbonization prepared in Comparative Example 2, wherein the upper left corners are marked as (a) and (b) are scanning electron microscope morphology images, and the images located below (a) and (b) are all Figure (c), and Figure (c) is an EDS image; wherein, Figures (a) and (b) show scanning electron microscope morphology images of H-DS at different magnification scales, and it can be seen that its morphology still retains a flaky structure and is smoother than the biomass carbon (DS) derived from pure durian shell. It can be clearly observed from the EDS distribution diagram of Figure (c) that the material contains only C and O elements, indicating that the hydrothermal pickling has achieved the purpose of removing impurities.
[0073] Figure 7 This is the XRD diffraction pattern of the pure durian shell-derived hard carbon material (H-DS) obtained after hydrothermal pickling and high-temperature carbonization prepared in Comparative Example 2. It can be seen that the XRD of H-DS has strong diffraction peaks at 2θ=23.27° and 43.08°, corresponding to the (002) and (101) crystal planes of the hard carbon material (standard card PDF#75-1621), indicating that the impurity peak disappears, that is, the pickling is effective in removing impurities, and the broad peak at about 23° indicates that the degree of graphitization is low, which is a typical characteristic of hard carbon materials.
[0074] Figure 8 The scanning electron microscope morphology and EDS spectrum of the hard carbon material (DS) derived from pure durian shell obtained by high-temperature carbonization without acid washing prepared in Comparative Example 3, wherein the upper left corners are marked as (a) and (b) are scanning electron microscope morphology images, and the images below (a) and (b) are all Figure (c), and Figure (c) is an EDS image; wherein Figures (a) and (b) show scanning electron microscope morphology images of DS at different magnification scales, and it can be seen that its morphology is mostly flaky, with a rich pore structure and a rough surface. It can be clearly observed from the EDS distribution diagram of Figure (c) that the prepared material contains more metal impurities.
[0075] Fig. 9 This is the XRD diffraction pattern of the pure durian shell-derived hard carbon material (DS) prepared in Comparative Example 3 without acid washing and only after high-temperature carbonization. It can be seen that the XRD of DS has strong diffraction peaks at 2θ=23.21° and 42.96°, corresponding to the (002) and (101) crystal planes of the hard carbon material (standard card PDF#75-1621), and the carbon diffraction peak is relatively broad. In addition to the carbon peak, there are other obvious impurity peaks, which are attributed to the metal impurities Mg and K in the material, that is, the pure durian shell-derived biomass carbon itself contains more impurities.
[0076] The nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material (NS-DS) prepared in Example 1, the nitrogen-doped durian shell-derived hard carbon material (N-DS) prepared in Comparative Example 1, the pure durian shell-derived hard carbon material (H-DS) obtained after hydrothermal pickling and high-temperature carbonization prepared in Comparative Example 2, and the pure durian shell-derived hard carbon material (DS) obtained after high-temperature carbonization without pickling prepared in Comparative Example 3 were used as negative electrode materials for sodium ion batteries, respectively, and rate performance tests were carried out. The use of the above materials as negative electrode materials for sodium ion batteries for rate performance tests belongs to the prior art and will not be repeated here. The test results are as follows: Fig.10 , 11 As shown in Figures 12 and 13, it can be seen that at a current density of 0.1C, the first discharge capacity of the NS-DS negative electrode material is as high as 246.1mAh / g, and the first efficiency exceeds 86%. Even at a high current density of 5C, the discharge capacity is still 60.1mAh / g, showing the best capacity and rate performance; at a current density of 0.1C, the first discharge capacity of the N-DS negative electrode material is 214.8mAh / g, and at a high current density of 5C, the discharge capacity is close to 57.7mAh / g, showing good capacity and rate performance; at a current density of 0. At 1C current density, the first discharge capacity of H-DS negative electrode material is 176.3mAh / g, and the first efficiency is 63.5%. At 5C high current density, the discharge capacity approaches 44.7mAh / g. Compared with DS negative electrode material, its performance has been improved accordingly, but it still shows poor capacity and rate performance; at 0.1C current density, the first discharge capacity of DS negative electrode material is only 138.7mAh / g, and the first efficiency is only 50.3%. At 5C high current density, the discharge capacity is only 5.4mAh / g, showing very poor capacity and rate performance. This confirms that functional modification by heteroatom doping has a significant effect on improving the sodium storage performance of biomass-derived hard carbon materials.
[0077] The above is only an embodiment of the present invention, and does not limit the present invention in any form. The present invention can also have other forms of embodiments according to the above structures and functions, which are not listed one by one. Therefore, any simple modification, equivalent change and modification made by any technician familiar with the profession to the above embodiment according to the technical essence of the present invention without departing from the scope of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A method for preparing a nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material, characterized in that: The specific steps include: (1) Pretreatment: drying and crushing the durian shell to millimeter level to obtain durian shell solid particles; (2) hydrothermal pickling: placing the durian shell solid particles obtained in step (1) in a hydrothermal kettle A, adding an acid solution, and then placing the hydrothermal kettle A in a forced air drying oven for hydrothermal pickling treatment, followed by cooling to room temperature, filtering the obtained product, washing with water until neutral, and then drying to obtain a durian shell-derived carbon precursor; (3) Hydrothermal doping: placing the carbon precursor derived from durian shell obtained in step (2) in a hydrothermal reactor B, adding an aqueous solution of ammonium sulfide, placing the hydrothermal reactor B in a forced air drying oven for hydrothermal doping treatment, and then cooling to room temperature, filtering and drying the obtained product to obtain a doped and modified carbon precursor intermediate; (4) High temperature carbonization: placing the doped and modified carbon precursor intermediate obtained in step (3) in a tube furnace and subjecting it to high temperature carbonization treatment in an inert atmosphere, cooling it naturally to room temperature, and finely grinding the obtained product to obtain a nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material.
2. The method for preparing the nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material as claimed in claim 1, characterized in that: The drying in step (1) is blast drying, the blast drying temperature is 50-100° C., and the drying time is 12-36 hours; the pulverizing is performed by a wall breaker, the power of the wall breaker is 900-3000W, the rotation speed is 20000-45000r / min, and the powder particle size after crushing is between 0.1 and 0.4mm.
3. The method for preparing the nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material as claimed in claim 1, characterized in that: The acid in the acid solution in step (2) includes but is not limited to one of sulfuric acid, hydrochloric acid and phosphoric acid, and the concentration of the acid solution is 0.01-1.0 mol / L; the mass ratio of the durian shell solid particles to the acid solution is 1:4-20.
4. The method for preparing the nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material as claimed in claim 1, characterized in that: After the acid solution is added to the hydrothermal kettle A in step (2), the filling rate of the hydrothermal kettle A is 50%-90%, the reaction temperature of the hydrothermal pickling treatment is 100-180°C, and the reaction time is 2-8h.
5. The method for preparing the nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material as claimed in claim 1, characterized in that: After the ammonium sulfide aqueous solution is added to the hydrothermal kettle B in step (3), the filling rate of the hydrothermal kettle B is 50%-90%; the reaction time of the hydrothermal doping treatment is 2-8 hours, and the reaction temperature is 180-250° C.; the concentration of the ammonium sulfide aqueous solution is 0.01-1.0 mol / L; and the mass ratio of the durian shell-derived carbon precursor to the ammonium sulfide solution is 1:5-20.
6. The method for preparing the nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material as claimed in claim 1, characterized in that: The inert atmosphere in step (4) is one of argon or nitrogen, and the inert atmosphere flow rate is 100 to 200 sccm; the high-temperature carbonization treatment is specifically to raise the temperature of the tubular furnace from room temperature to 800 to 1200°C and keep it warm for 2 to 4 hours at a heating rate of 5°C / min, and naturally cool to room temperature after the insulation is completed.
7. The method for preparing the nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material as claimed in claim 1, characterized in that: The fine grinding in step (4) is to dry-mill the obtained product in a ball mill and grind it to the micron level, and after fine grinding, the obtained powder is passed through a 500-mesh sieve to obtain a nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material.
8. The method for preparing the nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material as claimed in claim 7, characterized in that: In step (4), the obtained product is placed in an agate jar for dry ball milling, the mass ratio of agate balls to the obtained product is maintained at 20:1, the ball mill is operated at 200-400 rpm for 3-6 hours, and the rotation direction is reversed every 60 minutes.
9. The nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the nitrogen-sulfur co-doped functionalized durian shell-derived hard carbon material as claimed in claim 9 as a negative electrode material for sodium ion batteries.
Citation Information
Patent Citations
Post-treatment process for preparing super-capacitor active carbon with super-low ash content
CN102502621A
Spherical long-cycle stable biomass hard carbon material, preparation method and application
CN116161640A
Porous nitrogen-doped biomass nutshell hard carbon negative electrode material and preparation method thereof
CN116715218A