Waste tire rubber hard carbon material for negative electrode of sodium ion battery as well as preparation method and application of waste tire rubber hard carbon material
Through acidic solution pickling and zinc-containing compound ball milling, a waste tire rubber hard carbon material with a graphite microcrystalline structure and zinc single-atom doped active sites was prepared, which solved the lack of qualitative analysis of raw materials in the preparation of sodium-ion battery anode materials. It solves the problem of complex impurity removal process, achieves high reversible specific capacity and stable cycle performance, is suitable for sodium-ion battery negative electrode, and reduces cost.
Patent Information
- Application Number
- CN202411117122.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-10-29
AI Technical Summary
The preparation of existing hard carbon anode materials for sodium-ion batteries suffers from insufficient qualitative analysis of raw materials and unstable chemical compositions, which makes it difficult to achieve stable large-scale mass production, and the subsequent impurity removal process is complex, and the disclosed sulfur-doped porous carbon materials are used for Supercapacitors have low capacitance and cannot meet the standard use requirements of sodium-ion battery anode materials.
The waste tire rubber is pickled with an acidic solution, combined with zinc-containing compounds for ball milling and sintering, to prepare a waste tire rubber hard carbon material with a graphite microcrystalline structure and zinc single-atom doped active sites. Rubber carbon is generated through high-temperature sintering and Improve electrical conductivity.
The high reversible specific capacity and stable cycle performance of the waste tire rubber hard carbon material are achieved, and it is suitable for sodium-ion battery anodes. It is easy to operate and has low cost. It improves the resource utilization rate of waste tires and provides cheap and sustainable raw materials.
Smart Images

Figure CN118851156A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of battery materials, and particularly relates to a waste tire rubber hard carbon material for a negative electrode of a sodium ion battery, and a preparation method and application thereof. Background Art
[0002] As lithium-ion batteries are widely used in various electronic products such as electric vehicles, mobile phones, computers, etc., the demand for lithium is increasing year by year. However, the global lithium storage capacity is extremely limited, unevenly distributed, and costly, which seriously restricts the development of low-cost, high-performance energy storage devices. Sodium and lithium are elements of the same family. Sodium has similar electrochemical properties to lithium, and has abundant reserves and low costs. Therefore, sodium-ion batteries are the next generation of commercially applicable secondary batteries after lithium-ion batteries.
[0003] At present, the preparation of hard carbon negative electrode materials for sodium ion batteries mainly uses biomass such as coconut shells, straw, pollen, and bamboo as precursors. Hard carbon materials are obtained through steps such as water washing, calcination, oxidation, and secondary sintering as negative electrode materials for sodium ion batteries. Due to the lack of qualitative analysis of raw materials and the possible differences in chemical composition of raw materials from different sources, and the chemical composition of raw materials is not fixed, it is difficult to achieve stable large-scale mass production, and the subsequent impurity removal process is also relatively complicated.
[0004] As a rich resource, waste tire rubber has potential value in the preparation of hard carbon negative electrode materials. The main components of waste tire rubber are natural rubber and synthetic rubber (such as styrene-butadiene rubber, butadiene rubber, isoprene rubber, etc.), and also contain additives such as carbon black, sulfur, iron oxide, silicon oxide, and calcium oxide. Therefore, waste tire rubber can be converted into hard carbon materials through appropriate treatment methods. This conversion can not only effectively recycle waste tire resources and reduce environmental pollution, but also provide excellent performance negative electrode materials for sodium ion batteries.
[0005] The Chinese patent with publication number CN113213451A discloses an efficient carbon-rich waste tire resource processing method. The patent mixes the pickled rubber with zinc chloride for pyrolysis to obtain pyrolysis oil and pyrolysis coke, and then mixes the pyrolysis coke with sodium hydroxide for activation, pickling and purification to obtain sulfur-doped porous carbon. The patent uses alkali-assisted activation to treat waste tires, and the pore volume of the sulfur-doped porous carbon material obtained is too large. In addition, the sulfur-doped porous carbon material disclosed in the patent has a low specific capacitance when used in supercapacitors and cannot meet the standard use requirements of negative electrode materials for sodium ion batteries. Summary of the invention
[0006] In view of this, the object of the present invention is to provide a waste tire rubber hard carbon material for the negative electrode of a sodium ion battery and a preparation method and application thereof. The waste tire rubber hard carbon material provided by the present invention is used for the negative electrode of a sodium ion battery, showing the advantages of high reversible specific capacity and stable cycle performance.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] A method for preparing a waste tire rubber hard carbon material comprises the following steps:
[0009] washing the waste tire rubber with an acid solution to obtain pretreated waste tire rubber;
[0010] The pretreated waste tire rubber is mixed with a doping component precursor, and ball milled and sintered in sequence to obtain the waste tire rubber hard carbon material;
[0011] The doping component precursor is a zinc-containing compound;
[0012] The sintering temperature is 700-1500°C.
[0013] Preferably, the waste tire rubber includes one or more mixtures of natural rubber, styrene-butadiene rubber, butadiene rubber and isoprene rubber.
[0014] Preferably, the acidic solution comprises one of dilute hydrochloric acid solution, dilute sulfuric acid solution or dilute nitric acid solution; the concentration of the acidic solution is 0.1-1 mol / L; the dosage ratio of the waste tire rubber to the acidic solution is 1 g:10-50 mL.
[0015] Preferably, the pickling is carried out under boiling conditions; the pickling time is 0.5 to 5 hours.
[0016] Preferably, the zinc-containing compound includes one or more of zinc chloride, zinc acrylate and zinc gluconate; and the mass ratio of the pretreated waste tire rubber to the doping component precursor is 1 to 4:1.
[0017] Preferably, the ball milling process is performed at a speed of 300 to 500 r / min and for a time of 1 to 5 h;
[0018] The sintering time is 1 to 8 hours, the heating rate to the sintering temperature is 5 to 20° C. / min, and the atmosphere is argon.
[0019] The present invention also provides a waste tire rubber hard carbon material prepared by the preparation method described in the above technical scheme, wherein the waste tire rubber hard carbon material comprises a matrix and a doping component loaded on the matrix; the matrix is rubber hard carbon; the rubber hard carbon is the carbon-containing material obtained after sintering the waste tire rubber described in claim 1; and the doping component is a single zinc atom.
[0020] Preferably, the particle size of the waste rubber and waste tire rubber hard carbon material is 1 to 200 μm.
[0021] The present invention also provides a waste tire rubber hard carbon material prepared by the preparation method described in the above technical solution or the use of the waste tire rubber hard carbon material in a negative electrode of a sodium ion battery.
[0022] The invention provides a method for preparing a waste tire rubber hard carbon material, comprising the following steps: using an acid solution to pickle the waste tire rubber to obtain pretreated waste tire rubber; mixing the pretreated waste tire rubber with a doping component precursor, and sequentially performing ball milling treatment and sintering to obtain the waste tire rubber hard carbon material; the doping component precursor is a zinc-containing compound; and the sintering temperature is 700-1500°C.
[0023] The present invention uses an acid solution to pickle the waste tire rubber, which can effectively remove inorganic components and impurities in the waste tire rubber, and at the same time facilitates the doping component precursor to penetrate into the waste tire rubber, which is beneficial to the mixing of the two substances. The present invention mixes the pretreated waste tire rubber with the doping component precursor, and sequentially performs ball milling and sintering. The ball milling process makes the pretreated waste tire rubber and the doping component precursor more uniformly mixed, and at the same time controls the particle size and component uniformity of the particles, so that the waste tire rubber hard carbon material is more suitable for preparing sodium ion batteries. The present invention sintered the mixture of pretreated waste tire rubber after ball milling and the doping component precursor at 700-1500°C, so as to generate rubber carbon from the waste tire rubber. The waste tire rubber hard carbon material prepared by the embodiment of the present invention was tested by XRD, and there were two obvious carbon peaks at 2θ=24° and 44°, corresponding to the (002) and (100) graphite planes, indicating that the waste tire rubber hard carbon material prepared by the present invention had a graphite microcrystal-like graphite structure, which was more conducive to the embedding, migration and release of sodium ions. On the other hand, the rubber carbon at high temperature was reducing, and the zinc compound of the doping component precursor was reduced to zinc single atoms, thereby forming doping active sites in the matrix of the waste tire rubber hard carbon material, improving the conductivity of the waste tire rubber hard carbon material, and obtaining the waste tire rubber hard carbon material with high reversible specific capacity. In addition, the preparation method provided by the present invention is easy to operate, and the raw materials of the waste tire rubber used are widely available and low in cost, which improves the resource utilization of the waste tire rubber, greatly improves the utilization rate of the waste tire rubber, effectively reduces the cost, and can also provide cheap and sustainable raw materials for sodium ion battery materials. The prepared waste tire rubber hard carbon material has excellent performance and has considerable market application prospects.
[0024] The present invention provides a waste tire rubber hard carbon material prepared by the above technical solution, wherein the waste tire rubber hard carbon material comprises a matrix and a doping component loaded on the matrix; the matrix is rubber hard carbon; the rubber hard carbon is a carbon-containing material obtained after sintering waste tire rubber; and the doping component is a zinc single atom. In the present invention, the doping component zinc single atom has the function of improving the conductivity of the material, and the zinc single atom is uniformly loaded on the rubber hard carbon matrix, embedded in the pores and interlayers of the rubber hard carbon, which helps to attract sodium ions into the pores and interlayers of the rubber hard carbon, and makes the sodium ions more evenly distributed, thereby improving the reversible specific capacity of the negative electrode material prepared with the waste tire rubber hard carbon material as a raw material. The waste tire rubber hard carbon material prepared by the present invention using waste tire rubber is uniformly dispersed, does not agglomerate, and has a high reversible specific capacity. The results of the embodiment show that the waste tire rubber hard carbon material provided by the present invention has a reversible specific capacity of 284mAh / g as a negative electrode of a sodium ion battery, which can not only be used for a negative electrode of a sodium ion battery with ordinary performance, but also meet the requirements of a negative electrode of a high-performance sodium ion battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 A flow chart of the method for preparing the waste tire rubber hard carbon material provided by the present invention;
[0026] Figure 2 This is a SEM image of the waste tire rubber hard carbon material prepared in Example 1;
[0027] Figure 3 This is the EDS graph of carbon element in the waste tire rubber hard carbon material prepared in Example 1;
[0028] Figure 4 This is the EDS graph of zinc element in the waste tire rubber hard carbon material prepared in Example 1;
[0029] Figure 5 This is the XRD pattern of the waste tire rubber hard carbon material prepared in Example 1;
[0030] Figure 6 The graph is a constant current charge and discharge test curve of the waste tire rubber hard carbon material prepared in Examples 1 to 6 and Comparative Example 1 as the negative electrode of a sodium ion battery. DETAILED DESCRIPTION
[0031] Figure 1 The process flow chart of the preparation method of the waste tire rubber hard carbon material provided by the present invention is as follows: Figure 1 The preparation method provided by the present invention is described.
[0032] The present invention provides a method for preparing a waste tire rubber hard carbon material, comprising the following steps:
[0033] washing the waste tire rubber with an acid solution to obtain pretreated waste tire rubber;
[0034] The pretreated waste tire rubber is mixed with a doping component precursor, and ball milled and sintered in sequence to obtain the waste tire rubber hard carbon material;
[0035] The doping component precursor is a zinc-containing compound;
[0036] The sintering temperature is 700-1500°C.
[0037] In the present invention, unless otherwise specified, the raw materials used in the present invention are preferably commercially available products.
[0038] The invention uses an acid solution to pickle the waste tire rubber to obtain the pretreated waste tire rubber.
[0039] In the present invention, the waste tire rubber preferably includes one or more mixtures of natural rubber, styrene-butadiene rubber, butadiene rubber and isoprene rubber.
[0040] In the present invention, the acidic solution preferably includes one of dilute hydrochloric acid solution, dilute sulfuric acid solution or dilute nitric acid solution, and more preferably dilute hydrochloric acid solution. In the present invention, the concentration of the acidic solution is preferably 0.1 to 1 mol / L.
[0041] In the present invention, the usage ratio of the waste tire rubber to the acidic solution is preferably 1 g: 10 to 50 mL, more preferably 1 g: 10 to 40 mL.
[0042] In the present invention, the pickling is preferably carried out under boiling conditions. In the present invention, the pickling time is preferably 0.5 to 5 hours, more preferably 2 hours.
[0043] After the acid washing, the present invention preferably further comprises hot filtration and drying. In the present invention, the drying temperature is preferably 50-80°C, more preferably 60°C; the drying time is preferably 20-36h, more preferably 24h.
[0044] The present invention adopts acid solution to pickle the waste tire rubber, which can effectively remove inorganic components and impurities in the waste tire rubber. At the same time, the acid solution corrodes the waste tire rubber, forming pores in the waste tire rubber matrix, which is conducive to the infiltration of the doping component precursor into the waste tire rubber. The pretreated waste tire rubber obtained by the present invention has the characteristics of no impurities and multiple pores.
[0045] After obtaining the pretreated waste tire rubber, the present invention mixes the pretreated waste tire rubber with a doping component precursor, and sequentially performs ball milling and sintering to obtain the waste tire rubber hard carbon material; the sintering temperature is 700-1500°C.
[0046] In the present invention, the doping component precursor is a zinc-containing compound, and the zinc-containing compound preferably includes one or more of zinc chloride, zinc acrylate and zinc gluconate, and more preferably zinc chloride.
[0047] In the present invention, the mass ratio of the pretreated waste tire rubber to the doping component precursor is preferably 1-4:1, more preferably 1-3:1, further preferably 1-2:1; and further preferably 1:1.
[0048] In the present invention, the rotation speed of the ball milling treatment is preferably 300 to 500 r / min, more preferably 300 r / min, and the time is preferably 1 to 5 h, more preferably 2 h.
[0049] The present invention adopts ball milling treatment to make the pretreated waste tire rubber and the doping component precursor mixed more evenly, and at the same time controls the particle size and component uniformity of the particles, so that the waste tire rubber hard carbon material is more suitable for preparing sodium ion batteries.
[0050] In the present invention, the sintering temperature is 700-1500°C, preferably 900-1500°C, and more preferably 900-1200°C. In the present invention, the sintering time is preferably 1-8h, more preferably 1-3h, and more preferably 2h. In the present invention, the heating rate to the sintering temperature is preferably 5-20°C / min, more preferably 5°C / min. In the present invention, the sintering is preferably carried out in an argon atmosphere.
[0051] The present invention sintered the mixture of pretreated waste tire rubber after ball milling and a doping component precursor, which can generate rubber carbon from the waste tire rubber on the one hand, and on the other hand, the rubber carbon at high temperature has reducing property, and the doping component precursor zinc compound is reduced into zinc single atom, thereby forming doping active sites in the waste tire rubber hard carbon material matrix, improving the conductivity of the waste tire rubber hard carbon material, and obtaining the waste tire rubber hard carbon material with high reversible specific capacity.
[0052] After the sintering, the present invention preferably further comprises washing and drying. In the present invention, the washing agent preferably comprises deionized water. In the present invention, the drying temperature is preferably 50 to 80° C., and the drying time is preferably 8 to 36 hours.
[0053] The present invention provides a waste tire rubber hard carbon material prepared by the above-mentioned preparation method, wherein the waste tire rubber hard carbon material comprises a matrix and a doping component loaded on the matrix; the matrix is rubber hard carbon; the rubber hard carbon is a carbon-containing material obtained after sintering the waste tire rubber described in the above-mentioned technical solution; and the doping component is a single zinc atom.
[0054] In the present invention, the particle size of the waste rubber and waste tire rubber hard carbon material is preferably 1 to 200 μm, more preferably 1 to 100 μm, and further preferably 1 to 50 μm.
[0055] In the present invention, the matrix of the waste tire rubber hard carbon material has the advantages of being free of impurities and being porous; the doping components have the advantages of improving the conductivity of the material and increasing the cycle life of the battery; the waste tire rubber hard carbon material provided by the present invention has the advantages of high reversible specific capacity and long cycle life.
[0056] The present invention also provides a waste tire rubber hard carbon material prepared by the preparation method described in the above technical solution or the use of the waste tire rubber hard carbon material in a negative electrode of a sodium ion battery.
[0057] The technical solution of the present invention is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0058] Example 1
[0059] 100 g of waste tire rubber (natural rubber) was added into 1000 mL of 1 mol / L dilute hydrochloric acid solution and boiled for 2 h. The solution was filtered while hot and the filtered solid was dried in an oven at 60° C. for 24 h to obtain pretreated waste tire rubber.
[0060] The pretreated waste tire rubber and zinc chloride were mixed evenly in a mass ratio of 1:1 and then placed in a ball mill at 300 r / min for 2 h.
[0061] The mixed system of pretreated waste tire rubber and zinc chloride after ball milling was placed in a porcelain boat for sintering at a sintering temperature of 1200°C, a heating rate of 5°C / min, and a time of 2h. The obtained product was washed with deionized water and dried to obtain a waste tire rubber hard carbon material.
[0062] Figure 2 This is the SEM image of the waste tire rubber hard carbon material prepared in Example 1. Figure 2 Magnified 5000 times, from Figure 2 It can be seen that the waste tire rubber hard carbon material prepared by the present invention has a loose and porous surface of hard carbon particles, and zinc is evenly distributed on the surface of the hard carbon material in a single-atom state, which is beneficial to the adsorption of sodium ions on the electrode surface.
[0063] Figure 3 This is the EDS graph of carbon element in the waste tire rubber hard carbon material prepared in Example 1. Figure 3 Magnified 5000 times, from Figure 3 It can be seen that the main component of the waste tire rubber hard carbon material prepared by the present invention is carbon. Figure 5 The information in is consistent.
[0064] Figure 4 This is the EDS graph of zinc element in the waste tire rubber hard carbon material prepared in Example 1. Figure 4 Magnified 5000 times, from Figure 4 It can be seen that the surface of the waste tire rubber hard carbon material prepared by the present invention has a small amount of zinc element but evenly distributed. Figure 5 The XRD image shows no diffraction peaks except for the two carbon peaks, indicating that the zinc in the hard carbon material of waste tire rubber exists in a single atomic state.
[0065] Figure 5 The XRD pattern of the waste tire rubber hard carbon material prepared in Example 1 is shown in FIG. Figure 5It can be seen that there are two obvious carbon peaks at 2θ=24° and 44°, corresponding to the (002) and (100) graphite planes, indicating that the waste tire rubber hard carbon material prepared by the present invention has graphite-like structures such as graphite crystallites, which is more conducive to the embedding, migration and release of sodium ions. When used as the negative electrode of a sodium ion battery, reversible storage of sodium can be achieved during the charging process.
[0066] Example 2
[0067] The only difference from Example 1 is that the sintering temperature is 900°C.
[0068] Example 3
[0069] The only difference from Example 1 is that the sintering temperature is 1500°C.
[0070] Example 4
[0071] The only difference from Example 1 is that the zinc chloride in Example 1 is replaced by zinc acrylate.
[0072] Example 5
[0073] The only difference from Example 1 is that the zinc chloride in Example 1 is replaced by zinc gluconate.
[0074] Example 6
[0075] The difference from Example 1 is that the zinc chloride in Example 1 is replaced by a mixture of zinc chloride and zinc gluconate, and the mass ratio of the pretreated waste tire rubber to the zinc chloride and the zinc gluconate is 2:1:1.
[0076] Comparative Example 1
[0077] The only difference from Example 1 is that no zinc chloride is added.
[0078] Test analysis
[0079] The metallic sodium sheet was used as the positive electrode, and the waste tire rubber hard carbon material prepared in Examples 1 to 6 and Comparative Example 1 was used as the negative electrode. The button sodium ion battery was assembled in a glove box filled with nitrogen and with a water oxygen index strictly controlled to be less than 11 ppm.
[0080] The electrochemical properties of the prepared button sodium ion battery were tested by the constant current charge and discharge method at a voltage of 0 to 3 V and a current density of 50 mA / g using the Xinwei battery test system, including the reversible specific capacity and the specific capacity of each constant current charge and discharge test (see Figure 6 ) and the specific capacity of the 100th constant current charge and discharge test, the test results are shown in Table 1;
[0081] The reversible specific capacity is the specific capacity after the constant current charge and discharge test runs smoothly. The calculation method is: the average value of the specific capacity of the 5th to 100th times during the constant current charge and discharge test. The test results are shown in Table 1.
[0082] Table 1 Test results of waste tire rubber hard carbon materials as negative electrodes prepared in Examples and Comparative Examples
[0083]
[0084] from Figure 6 It can be seen that the waste tire rubber hard carbon material obtained in Examples 1 to 6 and Comparative Example 1 as the negative electrode has a more serious capacity decay in the first 1 to 5 cycles of constant current charge and discharge, which is consistent with the common formation process of lithium-ion batteries. In the constant current charge and discharge process thereafter, the specific capacity decays very slowly. The specific capacity fluctuation of each constant current charge and discharge of Examples 1 to 3 is very small, indicating that the operation is stable, the resistance of the electrode and electrolyte interface is small, and the lithium ions and electrolyte enter or leave the negative electrode smoothly, which proves from the side that the waste tire rubber hard carbon material obtained in Examples 1 to 3 is dense and uniform; the specific capacity fluctuation of each constant current charge and discharge of Examples 4 to 6 is large, but the specific capacity is not lower than 80% of the reversible specific capacity, indicating that the waste tire rubber hard carbon material obtained in Examples 4 to 6 has higher electrical properties and specific capacity, but the stability is somewhat lacking, and the material processing process needs to be further optimized and improved.
[0085] It can be seen from Table 1 that the reversible specific capacity of Examples 1 to 6 of the present invention is higher than that of Comparative Example 1, indicating that the present invention doped zinc in the waste tire rubber carbon material, which is beneficial to improving the conductivity, specific capacity and reversible specific capacity of the material. The specific capacity of the 100th time of constant current charge and discharge of Examples 1 to 6 is also higher than that of Comparative Example 1, and the specific capacity of the 100th time of Examples 1 to 8 is higher than 80% of the reversible specific capacity, indicating that the waste tire rubber hard carbon material prepared by the present invention has good cycle charge and discharge performance as a negative electrode, and can still maintain a high specific capacity after repeated use. The waste tire rubber hard carbon material prepared by the present invention can meet the performance requirements as a high-performance sodium ion battery negative electrode material, and reuse waste tires as resources, greatly improving the utilization rate of tire carbon, effectively reducing costs, and can also provide a cheap and sustainable source of raw materials for sodium ion batteries.
[0086] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. A method for preparing a waste tire rubber hard carbon material, characterized in that: The following steps are involved: washing the waste tire rubber with an acid solution to obtain pretreated waste tire rubber; The pretreated waste tire rubber is mixed with a doping component precursor, and ball milled and sintered in sequence to obtain the waste tire rubber hard carbon material; The doping component precursor is a zinc-containing compound; The sintering temperature is 700-1500°C.
2. The preparation method according to claim 1, characterized in that: The waste tire rubber includes one or more mixtures of natural rubber, styrene-butadiene rubber, butadiene rubber and isoprene rubber.
3. The preparation method according to claim 1 or 2, characterized in that: The acidic solution includes one of dilute hydrochloric acid solution, dilute sulfuric acid solution or dilute nitric acid solution; the concentration of the acidic solution is 0.1-1 mol / L; the usage ratio of the waste tire rubber to the acidic solution is 1g:10-50mL.
4. The preparation method according to claim 1, characterized in that: The pickling is carried out under boiling conditions; the pickling time is 0.5 to 5 hours.
5. The preparation method according to claim 1, characterized in that: The zinc-containing compound includes one or more of zinc chloride, zinc acrylate and zinc gluconate; the mass ratio of the pretreated waste tire rubber to the doping component precursor is 1 to 4:
1.
6. The preparation method according to claim 1, characterized in that: The ball milling process is performed at a speed of 300 to 500 r / min and a time of 1 to 5 hours; The sintering time is 1 to 8 hours, the heating rate to the sintering temperature is 5 to 20° C. / min, and the atmosphere is argon.
7. The waste tire rubber hard carbon material prepared by the preparation method according to any one of claims 1 to 6, characterized in that: The waste tire rubber hard carbon material comprises a matrix and a doping component loaded on the matrix; the matrix is rubber hard carbon; the rubber hard carbon is the carbon-containing material obtained by sintering the waste tire rubber as described in claim 1; the doping component is a single zinc atom.
8. The waste tire rubber hard carbon material according to claim 7, characterized in that: The particle size of the waste rubber and waste tire rubber hard carbon material is 1 to 200 μm.
9. Use of the waste tire rubber hard carbon material prepared by the preparation method according to any one of claims 1 to 6 or the waste tire rubber hard carbon material according to any one of claims 7 to 8 in the negative electrode of a sodium ion battery.
Citation Information
Patent Citations
Efficient carbon-rich waste tire resourceful treatment method
CN113213451A
Method for preparing capacitor electrode material from waste tire pyrolytic carbon
CN102214516A
Preparation methods of hard carbon material and hard carbon / graphite composite
CN109761211A
Preparation method of high-rate and low-temperature-resistant hard carbon negative electrode material and application of high-rate and low-temperature-resistant hard carbon negative electrode material in sodium-ion battery
CN116161643A
Metal ion modified biomass hard carbon material as well as preparation method and application thereof
CN117894967A