Method for purifying diamond micro-powder

By using chemical reactions and physical separation methods of acidic solutions and cerium salts in diamond micropowder, the high-risk and high-cost problems in the existing technology are solved, and efficient, environmentally friendly and low-cost diamond micropowder purification is achieved, meeting the requirements of high purity and high cost. Low cost requirements.

CN118851170APending Publication Date: 2024-10-29ZHANGJIAKOU YUANSHI ADVANCED MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411065106.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing diamond micropowder purification methods use high-risk chemical reagents and high-cost high-temperature and high-pressure conditions, leading to environmental pollution and safety hazards, and high costs, making it difficult to meet the needs of high purity and low cost.

Method used

Use acidic solution (such as sulfuric acid, hydrochloric acid) combined with cerium salt (such as cerium ammonium sulfate or cerium ammonium nitrate) to remove impurities in the diamond powder through chemical reaction and physical separation, improve the purity, and wash with stirring, heating and pure water and other steps to achieve purification, reducing energy consumption and waste of raw materials.

Benefits of technology

It significantly improves the purity of diamond powder, reduces harmful substance emissions and safety hazards, reduces production costs, is suitable for high-end field applications, and has strong process controllability and flexibility, making it suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851170A_ABST
    Figure CN118851170A_ABST
Patent Text Reader

Abstract

The method for purifying the diamond micro-powder comprises the following steps: S1, crushing diamond to obtain the diamond micro-powder; s2, adding the diamond micro-powder obtained in the previous step into an acid solution, and uniformly mixing to obtain a micro-powder acid solution; s3, adding cerium salt into the micro-powder acidic solution obtained in the previous step, and uniformly mixing to obtain a solid-liquid mixed solution; s4, heating the solid-liquid mixed solution obtained in the previous step, and uniformly stirring and mixing at a high speed; s5, the solid-liquid mixed solution obtained after stirring and mixing in the last step is washed with pure water till the solid-liquid mixed solution is neutral, and diamond micro powder is separated out; and S6, after the diamond micro powder obtained in the previous step is dried at high temperature, pure diamond micro powder is obtained. Through the synergistic effect of chemical reaction and physical separation, impurities in the diamond micro-powder are efficiently removed, and the purity of the diamond micro-powder is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of diamond micropowder manufacturing, and in particular relates to a method for purifying diamond micropowder. Background Art

[0002] Diamond powder, as a representative of superhard materials, has shown wide application potential in high-tech fields due to its unique physical and chemical properties. These powders are mainly composed of pure carbon and have extremely high hardness, thermal conductivity and electrical insulation, making them key materials in the manufacture of precision grinding tools, advanced cutting tools, electronic component heat sinks, gemstone processing, optical components and medical implants. Especially in precision machining, semiconductor manufacturing and advanced materials science, the demand for high-purity diamond powder is growing, which puts higher requirements on the performance of products.

[0003] At present, diamond micropowder is generally obtained by crushing large-particle polycrystalline diamond, purifying, acid washing and sorting to obtain diamond micropowder with concentrated particle size. Common purification methods include HClO4 acid washing oxidation purification method and H2SO4+KMnO4 and other redox purification methods. The use of a large amount of strong acid will produce waste acid and toxic gas pollution, HClO4 is also explosive, and the cost is relatively high. There are also studies using dilute nitric acid high-pressure purification method (8-12MPa), which must be established on a complete acid vapor and gas collection and recycling system, but the method has high requirements on the corrosion resistance, high pressure and high temperature resistance of the equipment, and the cost is relatively high. Summary of the invention

[0004] The present invention aims to provide a method for purifying diamond micropowder, so as to solve the technical problem of purifying diamond micropowder at low cost while ensuring the safety of production.

[0005] To achieve the above object, the specific technical scheme of a method for purifying diamond micropowder of the present invention is as follows:

[0006] A method for purifying diamond micropowder comprises the following steps:

[0007] S1, crushing the diamonds and screening to obtain diamond powder;

[0008] S2, adding the diamond powder obtained in the previous step into the acidic solution and mixing them evenly to obtain a powder acidic solution;

[0009] S3, adding cerium salt to the micropowder acidic solution obtained in the previous step and mixing evenly to obtain a solid-liquid mixed solution;

[0010] S4, heating the solid-liquid mixed solution obtained in the previous step and stirring at high speed to mix uniformly;

[0011] S5, washing the solid-liquid mixed solution obtained after stirring and mixing in the previous step with pure water until it becomes neutral, and separating the diamond powder;

[0012] S6. Dry the diamond micropowder obtained in the previous step at high temperature to obtain pure diamond micropowder.

[0013] As a further improvement of the present invention, in S2, the diamond powder is uniformly mixed in the acid solution by a stirring device at a stirring speed of 100 to 140 r / min.

[0014] As a further improvement of the present invention, in S3, the cerium salt is uniformly mixed in the micro-powder acidic solution by a stirring device at a stirring speed of 100 to 140 r / min.

[0015] As a further improvement of the present invention, in S4, the solid-liquid mixed solution is heated to 70-150° C. and mixed evenly by a stirring device at a stirring speed of 230-250 r / min.

[0016] As a further improvement of the present invention, the solid-liquid mixed solution in S5 is washed with pure water and then the diamond powder is separated by centrifugal separation.

[0017] As a further improvement of the present invention, the solid-liquid mixed solution in S5 is washed with pure water until the pH value is 6-8.

[0018] As a further improvement of the present invention, the acidic solution is sulfuric acid, and the cerium salt is ammonium cerium sulfate;

[0019] The solid-liquid ratio of diamond powder to sulfuric acid solution in S2 is 1:1 to 1:1.1 W / V;

[0020] The mass ratio of ammonium cerium sulfate to diamond powder in S3 is 1:0.9 to 1:1.1;

[0021] The solid-liquid mixed solution in S4 is stirred and mixed at 75-85°C and at a stirring speed of 230-250 r / min for 1 hour;

[0022] In S6, the mixture is dried at 110 to 130° C. for 6 hours.

[0023] As a further improvement of the present invention, the acidic solution is hydrochloric acid, and the cerium salt is ammonium cerium nitrate;

[0024] The solid-liquid ratio of diamond powder to hydrochloric acid solution in S2 is 1:10-1:11 W / V;

[0025] The mass ratio of ammonium cerium nitrate to diamond powder in S3 is 1:19 to 1:21;

[0026] The solid-liquid mixed solution in S4 is stirred and mixed at 110-130°C and at a stirring speed of 230-250 r / min for 4 hours;

[0027] The diamond powder in S6 is dried at 170-190°C for 8 hours.

[0028] As a further improvement of the present invention, the acidic solution is one of sulfuric acid, hydrochloric acid and nitric acid, and the cerium salt is ammonium cerium sulfate or ammonium cerium nitrate.

[0029] Beneficial effects:

[0030] The use of acidic solution combined with specific cerium salts (ammonium cerium sulfate or ammonium cerium nitrate) can effectively remove impurities in diamond micropowder, especially metal impurities, thereby improving the purification efficiency. The purity of the resulting diamond micropowder is significantly improved, meeting the high standards required in high-end fields such as precision machining and semiconductor manufacturing.

[0031] By precisely controlling the acid solution concentration, solid-liquid ratio and temperature conditions, the emission of harmful substances is reduced, and the subsequent pure water washing and centrifugal separation steps ensure the cleanliness of the treatment process and reduce the impact on the environment.

[0032] This method avoids the use of high-risk chemical reagents and extreme conditions, such as high temperature and high pressure, thereby greatly reducing safety hazards during the operation and ensuring production safety.

[0033] By optimizing the stirring speed and time control, as well as the reasonable setting of solid-liquid ratio and mass ratio, this method reduces energy consumption and raw material waste, thereby reducing production costs while ensuring the purification effect.

[0034] The present invention provides two different acidic solutions (sulfuric acid and hydrochloric acid) and corresponding cerium salt solutions, which meet the requirements of different types of diamond micropowder purification and enhance the flexibility and practicability of the method.

[0035] Specific and detailed operating parameters, such as specific stirring speed and temperature range, ensure the uniformity and effectiveness of each step of the treatment, improve the controllability and repeatability of the overall process, and are suitable for large-scale production.

[0036] In summary, the present invention provides an efficient, environmentally friendly and cost-effective method for purifying diamond micropowder, which not only solves the problems of environmental pollution, safety risks and high costs existing in the prior art, but also improves the quality and market competitiveness of the final product, and has significant practical value and social and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is a schematic diagram of an electron microscope of diamond micropowder after purification by the purification method of the present invention;

[0038] Figure 2 This is a schematic diagram of the elemental analysis structure of diamond micropowder after purification;

[0039] Figure 3 Schematic diagram of Raman spectrum of purified diamond micropowder;

[0040] Figure 4 Schematic diagram of the energy spectrum of purified diamond powder. DETAILED DESCRIPTION

[0041] In order to better understand the purpose, structure and function of the present invention, a method for purifying diamond micropowder of the present invention is further described in detail below in conjunction with the accompanying drawings.

[0042] Embodiment 1:

[0043] A method for purifying diamond micropowder is to purify the diamond micropowder by adding cerium salt and acid solution. The principle is mainly based on the combination of chemical reaction and physical separation. Its core purpose is to efficiently remove metal impurities and other non-carbon elements attached to the diamond micropowder to improve the purity of the micropowder.

[0044] Diamond micropowder is soaked in a strong acid solution (sulfuric acid, hydrochloric acid or nitric acid). The acidic environment can dissolve metal impurities (such as catalyst metal residues) on the surface of diamond. These impurities are often coated on the surface of diamond particles during the synthetic diamond process.

[0045] The cerium salt (ammonium cerium sulfate or ammonium cerium nitrate) added subsequently plays the role of catalyst and complexing agent. The presence of cerium salt can accelerate the reaction of metal impurities with acid, help form metal complexes that are more soluble in water, or directly react with certain impurities to generate soluble products, making it easier to remove from the diamond surface.

[0046] High-speed stirring and heating are used to promote chemical reactions and improve the efficiency of impurity removal. Afterwards, pure water washing and centrifugal separation technology are used to separate the diamond powder from the solution containing impurities, further purify the diamond powder, and finally the wet diamond powder is dried at high temperature to evaporate all the water to ensure that dry and pure diamond powder is obtained.

[0047] In this embodiment, sulfuric acid and ammonium cerium sulfate are selected to purify diamond powder through the following steps:

[0048] 1. Select high-quality raw diamond materials, crush them finely using professional crushing equipment, and obtain diamond micropowder with uniform particle size through screening and grading. The particle size range is pre-set according to application requirements.

[0049] 2. At room temperature (20-40°C), slowly add diamond powder into the pre-prepared sulfuric acid solution and mix evenly at a stirring speed of 120r / min. The solid-liquid ratio of diamond powder to sulfuric acid solution is 1:1W / V. Ensure that the surface of each powder can contact the sulfuric acid solution to remove surface impurities and obtain a powder sulfuric acid solution.

[0050] 3. At room temperature, slowly add ammonium cerium sulfate powder to the powder sulfuric acid solution in a mass ratio of 1:1 with diamond powder and mix them evenly at a stirring speed of 120r / min to allow the ammonium cerium sulfate to react chemically with the impurities on the surface of the powder, further promoting the dissolution of the impurities to obtain a solid-liquid mixed solution.

[0051] 4. Heat the solid-liquid mixed solution to 80°C in a heating and stirring device, and stir and mix at a stirring speed of 240r / min for 1 hour to accelerate the chemical reaction process and ensure the effective removal of impurities.

[0052] 5. Let the solid-liquid mixed solution stand, wait for the diamond powder to settle, extract the upper solution, wash it with pure water 3 times until the pH value of the solution is about 7, and separate the diamond powder by centrifugation.

[0053] 6. Dry the separated diamond micropowder in a constant temperature drying oven at 120°C for 6 hours to ensure that the micropowder is completely dry, which also helps to further remove moisture and possible residual volatile substances to obtain pure diamond micropowder.

[0054] like Figure 1-4 As shown, the surface of the diamond powder purified by the above method is displayed by electron microscopy, and various testing methods such as elemental analysis, Raman and energy spectrum are used to illustrate that the strong oxidizing property of strong acid and cerium ions can remove non-diamond impurities to obtain pure micron-sized diamond powder.

[0055] Embodiment 2:

[0056] In this embodiment, hydrochloric acid and ammonium cerium nitrate are selected to purify diamond powder through the following steps:

[0057] 1. Select high-quality raw diamond materials, crush them finely using professional crushing equipment, and obtain diamond micropowder with uniform particle size through screening and grading. The particle size range is pre-set according to application requirements.

[0058] 2. At room temperature, slowly add diamond powder into the pre-prepared hydrochloric acid solution and mix evenly at a stirring speed of 120r / min. The solid-liquid ratio of diamond powder to hydrochloric acid solution is 1:10W / V. Ensure that the surface of each powder can contact the hydrochloric acid solution to remove surface impurities and obtain a powder hydrochloric acid solution.

[0059] 3. At room temperature, slowly add ammonium cerium nitrate powder to the diamond powder in a mass ratio of 1:20 into the powder hydrochloric acid solution and mix evenly at a stirring speed of 120r / min to allow the ammonium cerium nitrate to react chemically with the impurities on the surface of the powder, further promoting the dissolution of the impurities to obtain a solid-liquid mixed solution.

[0060] 4. Heat the solid-liquid mixed solution to 120°C in a heating and stirring device, and stir and mix at a stirring speed of 240r / min for 4 hours to accelerate the chemical reaction process and ensure the effective removal of impurities.

[0061] 5. Let the solid-liquid mixed solution stand until the diamond powder is precipitated, then extract the upper solution and wash it repeatedly with pure water 5 times until the pH value of the solution is about 7. Use centrifugal separation to separate the diamond powder.

[0062] 6. Dry the separated diamond micropowder in a constant temperature drying oven at 180°C for 8 hours to ensure that the micropowder is completely dry, which also helps to further remove moisture and possible residual volatile substances to obtain pure diamond micropowder.

[0063] The purification method of the above two embodiments directly acts on impurities through chemical reaction, and compared with traditional physical screening, purification efficiency is higher, and various types of impurities can be effectively removed. By controlling the amount of chemicals used and subsequent purification steps, the generation of hazardous waste can be reduced, which is conducive to environmental protection. Although it is related to the use of chemical reagents, by optimizing process parameters (such as acid concentration, temperature, stirring speed, etc.), while ensuring the purification effect, cost can be controlled, and it is suitable for industrial production. The impurity content of the diamond micropowder after purification is low, and the performances such as hardness and thermal conductivity are significantly improved, which is more suitable for high-performance applications, such as precision grinding, advanced cutting tools, electronic components, etc. The whole process is easy to control through standardized operation, and by physical means such as centrifugation, the post-processing steps are simplified, and it is easy to realize automated production.

[0064] It is to be understood that the present invention is described by some embodiments, and it is known to those skilled in the art that various changes or equivalent substitutions may be made to these features and embodiments without departing from the spirit and scope of the present invention. In addition, under the teachings of the present invention, these features and embodiments may be modified to adapt to specific circumstances and materials without departing from the spirit and scope of the present invention. Therefore, the present invention is not limited by the specific embodiments disclosed herein, and all embodiments falling within the scope of the claims of this application are within the scope of protection of the present invention.

Claims

1. A method for purifying diamond micropowder, characterized in that: The following steps are involved: S1, crushing the diamonds and screening to obtain diamond powder; S2, adding the diamond powder obtained in the previous step into the acidic solution and mixing them evenly to obtain a powder acidic solution; S3, adding cerium salt to the micropowder acidic solution obtained in the previous step and mixing evenly to obtain a solid-liquid mixed solution; S4, heating the solid-liquid mixed solution obtained in the previous step and stirring at high speed to mix uniformly; S5, washing the solid-liquid mixed solution obtained after stirring and mixing in the previous step with pure water until it becomes neutral, and separating the diamond powder; S6. Dry the diamond micropowder obtained in the previous step at high temperature to obtain pure diamond micropowder.

2. The method for purifying diamond micropowder according to claim 1, characterized in that: In S2, the diamond powder is uniformly mixed in the acid solution by a stirring device at a stirring speed of 100 to 140 r / min.

3. The method for purifying diamond micropowder according to claim 2, characterized in that: In S3, the cerium salt is uniformly mixed in the fine powder acid solution at a stirring speed of 100 to 140 r / min by a stirring device.

4. The method for purifying diamond micropowder according to claim 3, characterized in that: In S4, the solid-liquid mixed solution is heated to 70-150° C. and mixed uniformly at a stirring speed of 230-250 r / min by a stirring device.

5. The method for purifying diamond micropowder according to claim 4, characterized in that: The solid-liquid mixed solution in S5 is washed with pure water and then the diamond powder is separated by centrifugation.

6. The method for purifying diamond micropowder according to claim 1, characterized in that: The solid-liquid mixed solution in S5 is washed with pure water to a pH value of 6-8.

7. The method for purifying diamond micropowder according to claim 5, characterized in that: The acidic solution is sulfuric acid, and the cerium salt is ammonium cerium sulfate; The solid-liquid ratio of diamond powder to sulfuric acid solution in S2 is 1:1 to 1:1.1 W / V; The mass ratio of ammonium cerium sulfate to diamond powder in S3 is 1:0.9 to 1:1.1; The solid-liquid mixed solution in S4 is stirred and mixed at 75-85°C and at a stirring speed of 230-250 r / min for 1 hour; In S6, the mixture is dried at 110 to 130° C. for 6 hours.

8. The method for purifying diamond micropowder according to claim 5, characterized in that: The acidic solution is hydrochloric acid, and the cerium salt is ammonium cerium nitrate; The solid-liquid ratio of diamond powder to hydrochloric acid solution in S2 is 1:10-1:11 W / V; The mass ratio of ammonium cerium nitrate to diamond powder in S3 is 1:19 to 1:21; The solid-liquid mixed solution in S4 is stirred and mixed at 110-130° C. and at a stirring speed of 230-250 r / min for 4 hours; The diamond powder in S6 is dried at 170-190°C for 8 hours.

9. The method for purifying diamond micropowder according to claim 1, characterized in that: The acid solution is one of sulfuric acid, hydrochloric acid and nitric acid, and the cerium salt is ammonium cerium sulfate or ammonium cerium nitrate.

Citation Information

Patent Citations

  • Method of purifying environment-friendly type ultra-fine diamond

    CN101033065A

  • Method for producing nano diamond particles purified by cerium salt

    CN1480252A

  • Method for refining superfine artificial diamond

    CN1693188A