Kaolin full-resource utilization method
By grinding and activating kaolin and treating it with sulfuric acid solution, combined with adsorption resin and lime to adjust the pH value, the extraction of gallium and the separation of major elements were successfully achieved, solving the problem of full resource utilization of kaolin resources and improving the utilization value. and economic benefits.
Patent Information
- Application Number
- CN202410807802.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-21
AI Technical Summary
At present, there is no efficient technology that can simultaneously extract gallium from kaolin and achieve full resource utilization of its major elements, including the extraction of alumina, silica powder and iron oxide.
By grinding and activating kaolin, then dissolving it in a sulfuric acid solution and using adsorption resin to adsorb gallium ions, adjusting the pH value with lime, separating and calcining it to obtain products such as alumina, calcium sulfate and iron oxide, achieving full utilization of resources.
It improves the overall utilization value of kaolin, has a high recovery rate, no secondary waste emissions, good economic benefits, and is easy to implement industrialization.
Smart Images

Figure CN118851186A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of comprehensive utilization of mineral resources, and in particular to a method for comprehensive resource utilization of kaolin. Background Art
[0002] Gallium is an important rare metal, which is widely used in the manufacture of solar photovoltaic cells, light-emitting diodes, etc. Gallium generally does not exist in independent deposits, and is mainly associated with other mineral resources. In recent years, studies have found that in addition to the main elements aluminum, iron and silicon, kaolin in Shanxi, Inner Mongolia and other places in my country also has relatively rich gallium resources, with a gallium content of 12 to 230 μg / g, which has important utilization value. However, there is currently no technology to extract gallium from kaolin while fully utilizing its main elements. Summary of the invention
[0003] Based on the above situation, the main purpose of the present invention is to provide a method for the full resource utilization of kaolin, which can not only efficiently extract the valuable metal gallium in kaolin, but also extract components such as aluminum silicon and iron into aluminum oxide, silicon powder, and iron oxide, thereby realizing the full resource utilization of kaolin.
[0004] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0005] The present invention provides a method for fully utilizing kaolin resources, comprising the following steps:
[0006] S100, grinding kaolin to a particle size of 50-90 μm, activating at a temperature of 200-700° C. for 30-60 min, and obtaining sample M;
[0007] S200, placing the sample M in a first sulfuric acid solution with a concentration of 1 to 6 mol / L at a temperature of 40 to 90° C. at a liquid-to-solid ratio of 4 to 10, stirring and dissolving for 30 to 90 minutes, and then filtering to obtain silicon micropowder and filtrate A;
[0008] S300, adsorbing gallium ions with an adsorption resin at a temperature of 40 to 60° C. on the filtrate A, and obtaining a solution after adsorbing gallium as the filtrate B. After the gallium adsorption is completed, the resin is taken out, and eluted with a second sulfuric acid solution with a concentration of 2 to 3 mol / L at a temperature of 40 to 60° C. to obtain gallium sulfate;
[0009] S400, adding lime to the filtrate B at 40-60° C. to adjust the pH value of the filtrate B to between 2.5 and 3.3, monitoring the pH value of the filtrate B in real time, and when the pH value of the solution drops below 2.5, adding lime to return the pH value to 2.5-3.3, and filtering when no lime needs to be added and the pH value does not drop below 2.5 for more than 20 minutes, to obtain a mixture of ferric hydroxide and calcium sulfate and a filtrate C;
[0010] S500, dissolving the mixture of ferric hydroxide and calcium sulfate obtained in step S400 in a third sulfuric acid solution having a concentration of 2 to 4 mol / L at a temperature of 40 to 90° C. at a liquid-to-solid ratio of 3 to 7, reacting for 5 to 30 minutes, and filtering to obtain calcium sulfate and filtrate D;
[0011] S600, the filtrate C is crystallized to obtain aluminum sulfate, which is calcined at 750-850°C for 20-60min to obtain aluminum oxide and SO3, and the SO3 is recovered to make acid and then returned to the above reaction step for use;
[0012] S700, the filtrate D is crystallized to obtain ferric sulfate, which is calcined at 700-800°C for 20-60min to obtain iron oxide and SO3, and the SO3 is recovered and then returned to the above reaction step for use in acid production.
[0013] Preferably, in step S100, the particle size of the kaolin after grinding is preferably 74 μm, the activation temperature is preferably 600° C., and the activation time is preferably 40 min.
[0014] Preferably, in step S200, the liquid-to-solid ratio of the first sulfuric acid solution to the sample M is preferably 10, the temperature condition is preferably 70° C., the concentration of the first sulfuric acid solution is preferably 1.5 mol / L, and the stirring dissolution time is preferably 60 min.
[0015] Preferably, in step S300, the adsorption resin is LX-92 resin, CL-P204 leaching resin, IRA900 resin, and / or chelating resin.
[0016] Preferably, in step S300, gallium ions are adsorbed by an adsorption resin at a temperature of 50° C., and after the gallium-adsorbed resin is taken out, gallium sulfate is preferably eluted by a second sulfuric acid solution with a concentration of 3 mol / L at 60° C. for 20 to 60 min.
[0017] Preferably, in the step S400, lime is added to the filtrate B at 45° C., and the pH value of the filtrate is preferably controlled at 2.8.
[0018] Preferably, in step S500, the concentration of the third sulfuric acid solution is preferably 3 mol / L, the liquid-to-solid ratio of the third sulfuric acid solution to the mixture of ferric hydroxide and calcium sulfate is preferably 4, the temperature condition is preferably 75° C., and the reaction time is preferably 15 min.
[0019] Preferably, in step S600, the calcination temperature is preferably 800° C., and the calcination time is preferably 40 min.
[0020] Preferably, in step S700, the calcination temperature is preferably 750° C., and the calcination time is preferably 40 min.
[0021] The method for the full resource utilization of kaolin provided by the present invention not only recovers the valuable metal gallium in kaolin, but also separates and extracts other major components in kaolin into products such as aluminum oxide, silicon micropowder, and iron oxide. The lime added during the extraction process can also be converted into gypsum for subsequent industrial use. The method greatly improves the overall utilization value of kaolin, has the advantages of high recovery rate of valuable metals, no secondary waste discharge, good economic benefits, and easy industrialization, and opens up a new way for the resource utilization of kaolin.
[0022] Other beneficial effects of the present invention will be explained in the specific implementation manner through the introduction of specific technical features and technical solutions. Through the introduction of these technical features and technical solutions, those skilled in the art should be able to understand the beneficial technical effects brought about by the technical features and technical solutions. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The preferred embodiments of the present invention will be described below with reference to the accompanying drawings.
[0024] Figure 1 A flow chart of a preferred implementation of the method for full resource utilization of kaolin provided by the present invention;
[0025] Figure 2 The present invention is a flowchart of another preferred embodiment of the method for full resource utilization of kaolin provided by the present invention. DETAILED DESCRIPTION
[0026] The present invention is described below based on embodiments, but the present invention is not limited to these embodiments. In the following detailed description of the present invention, some specific details are described in detail. In order to avoid confusing the essence of the present invention, known methods, processes, procedures, and components are not described in detail.
[0027] In addition, persons of ordinary skill in the art will appreciate that the drawings provided herein are for illustration purposes and are not necessarily drawn to scale.
[0028] Unless the context clearly requires otherwise, throughout the specification and claims, the words "include", "comprising" and similar words should be interpreted in an inclusive sense rather than an exclusive or exhaustive sense; that is, in the sense of "including but not limited to".
[0029] In the description of the present invention, it should be understood that the terms "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance. In addition, in the description of the present invention, unless otherwise specified, "plurality" means two or more.
[0030] See attached Figure 1 The present invention provides a method for fully utilizing kaolin resources, comprising the following steps:
[0031] S100, grinding kaolin to a particle size of 50-90 μm, activating at a temperature of 200-700° C. for 30-60 min, and obtaining sample M;
[0032] S200, placing the sample M in a first sulfuric acid solution with a concentration of 1 to 6 mol / L at a temperature of 40 to 90° C. at a liquid-to-solid ratio of 4 to 10, stirring and dissolving for 30 to 90 minutes, and then filtering to obtain silicon micropowder and filtrate A;
[0033] S300, adsorbing gallium ions with an adsorption resin at a temperature of 40 to 60° C. on the filtrate A, and obtaining a solution after adsorbing gallium as the filtrate B. After the gallium adsorption is completed, the resin is taken out, and eluted with a second sulfuric acid solution with a concentration of 2 to 3 mol / L at a temperature of 40 to 60° C. to obtain gallium sulfate;
[0034] S400, adding lime to the filtrate B at 40-60° C. to adjust the pH value of the filtrate B to between 2.5 and 3.3, monitoring the pH value of the filtrate B in real time, and when the pH value of the solution drops below 2.5, adding lime to return the pH value to 2.5-3.3, and filtering when no lime needs to be added and the pH value does not drop below 2.5 for more than 20 minutes, to obtain a mixture of ferric hydroxide and calcium sulfate and a filtrate C;
[0035] S500, dissolving the mixture of ferric hydroxide and calcium sulfate obtained in step S400 in a third sulfuric acid solution having a concentration of 2 to 4 mol / L at a temperature of 40 to 90° C. at a liquid-to-solid ratio of 3 to 7, reacting for 5 to 30 minutes, and filtering to obtain calcium sulfate and filtrate D;
[0036] S600, the filtrate C is crystallized to obtain aluminum sulfate, which is calcined at 750-850° C. for 20-60 min to obtain aluminum oxide and SO3, and the SO3 is recovered to produce acid and then returned to the above reaction step for use;
[0037] S700, the filtrate D is crystallized to obtain ferric sulfate, which is calcined at 700-800°C for 20-60 min to obtain iron oxide and SO3, and the SO3 is recovered and returned to the above reaction step for use in acid production.
[0038] Specifically, the present invention first activates kaolin through step S100 before kaolin powder reacts with sulfuric acid (i.e., "acid leaching") to extract relevant elements for resource utilization. Through the activation process, kaolinite, the main component of kaolin, undergoes a dehydroxylation reaction to obtain sample M, which can greatly improve the reaction activity of the acid leaching reaction in step S200 and significantly improve the acid leaching reaction speed. Otherwise, the reaction speed of the reaction will be very slow, and the requirements for the concentration of the first sulfuric acid solution and the reaction temperature will be higher, which is not convenient for the preparation of the first sulfuric acid solution and the reaching of the reaction temperature.
[0039] Kaolinite is a mineral with the chemical formula of Al2O3·2SiO2·2H2O. In the activation step, its dehydroxylation reaction equation is as follows:
[0040] (amorphous)+2H2O↑
[0041] During the acid leaching process of step S200, the main components in the sample M react with the first sulfuric acid solution as follows:
[0042] Al2O3+3H2SO4=Al2(SO4)3+3H2O
[0043] Fe2O3+3H2SO4=Fe2(SO4)3+3H2O
[0044] Ga2O3+3H2SO4=Ga2(SO4)3+3H2O
[0045] Filtrate A contains aluminum sulfate, iron sulfate, and gallium sulfate;
[0046] In this step, the total amount of acid used is coordinated and controlled by preparing a suitable liquid-to-solid ratio between the sample M and the first sulfuric acid solution and a suitable concentration of the first sulfuric acid solution, so as to avoid the situation where the oxides cannot be completely dissolved when the acid is insufficient, resulting in residual oxides in the silicon micropowder and affecting the purity of the product; it also avoids the obvious excessive use of acid, which leads to an unnecessary increase in the amount of lime added in the pH adjustment process of the subsequent step S400.
[0047] Further considering that the temperature condition affects the reaction rate, the lower the temperature, the lower the reaction rate and the longer the reaction time; the higher the temperature, the higher the reaction rate and the shorter the reaction time, therefore in step S200, 40-90°C is selected as the appropriate temperature condition.
[0048] Then, the present invention obtains gallium sulfate through step S300. In this step, the temperature environment during adsorption is set between 40 and 60°C, which can make the adsorption rate of the adsorption resin to the gallium element relatively high. If the temperature is too high or too low relative to the aforementioned range, the adsorption capacity will be reduced. The principle of resin adsorption of gallium is selective ion exchange, and the adsorption reaction equation is as follows (where R represents organic resin):
[0049] Ga 3+ +3HR=GaR3+3H +
[0050] Usually, after 30 to 150 minutes, the gallium element can be completely adsorbed. After the resin that has completely adsorbed gallium is taken out, the resin that has adsorbed gallium undergoes a desorption reaction (i.e., the reverse process of the adsorption reaction) through the strong acidic medium conditions provided by the second sulfuric acid solution with a concentration of 2 to 3 mol / L, thereby obtaining gallium sulfate. The main reaction equation of the desorption reaction is as follows:
[0051] GaR3+3H + =Ga 3+ +3HR;
[0052] The gallium sulfate obtained after elution can be used as a raw material for the industrial production of gallium oxide and metallic gallium.
[0053] Next, the present invention obtains a mixture of ferric hydroxide and calcium sulfate and filtrate C through step S400, and then separates calcium and iron elements through steps S500 and S700 for extraction and utilization.
[0054] The present invention finds that by adding lime to the filtrate B at 40-60° C. and controlling the pH value of the filtrate to be between 2.5 and 3.3 (specifically, by adding lime to the filtrate B at 40-60° C. from step S300 to adjust the pH value of the filtrate B to between 2.5 and 3.3, and monitoring the pH value of the filtrate B in real time, and when the pH value of the solution drops below 2.5, adding lime to return the pH value to 2.5-3.3), the filtrate B can undergo the following reaction so that only the aluminum element to be extracted and utilized is left in the filtrate C:
[0055] CaO+2H + +SO4 2- =CaSO4↓+H2O
[0056] Fe 3+ +3OH - =Fe(OH)3↓
[0057] For the mixture of iron hydroxide and calcium sulfate obtained in step S400, the present invention performs step S500, adding the mixture to the third sulfuric acid solution so that the iron hydroxide reacts with the third sulfuric acid solution, and calcium sulfate (i.e., gypsum) is insoluble in the sulfuric acid solution and precipitates in the form of precipitation, and only the iron element to be extracted and utilized is left in the obtained filtrate D. The main reaction equation performed in step S500 is as follows:
[0058] 3H2SO4+2Fe(OH)3=Fe2(SO4)3+6H2O
[0059] At this time, the present invention performs step S700 on the filtrate D, crystallizes it to obtain ferric sulfate, calcines it to obtain ferric oxide and SO3, and recovers SO3 to make acid and then returns it to the above reaction step for use. The main reaction equation of this step is as follows:
[0060]
[0061] SO3+H2O=H2SO4
[0062] Through step S700, not only iron oxide that can be directly used as an industrial raw material can be obtained, but also SO3 can be obtained. It can be recycled to prepare the first sulfuric acid solution, the second sulfuric acid solution and / or the third sulfuric acid solution, which can be used in the subsequent cyclic process of full resource utilization of kaolin. This further reduces the amount of additional sulfuric acid added and significantly saves raw material input.
[0063] The present invention also performs step S600 to crystallize the filtrate C to obtain aluminum sulfate, calcine to obtain aluminum oxide and SO3, and the SO3 is also recovered and returned to the above reaction step for use after acid production. The main reaction equation of this step is as follows:
[0064]
[0065] SO3+H2O=H2SO4
[0066] It should be noted that the sequence of the present invention does not constitute a limitation on the actual operation steps. Unless a step requires the occurrence of the previous step as a prerequisite, the operation can be disrupted. For example, step S600 can be performed immediately after step S400, or immediately after step S500, or immediately after step S700.
[0067] The method for the full resource utilization of kaolin provided by the present invention not only recovers the valuable metal gallium in kaolin, but also separates and extracts other major components in kaolin into products such as aluminum oxide, silicon micropowder, and iron oxide. The lime added during the extraction process can also be converted into gypsum for subsequent industrial use. The method greatly improves the overall utilization value of kaolin, has the advantages of high recovery rate of valuable metals, no secondary waste discharge, good economic benefits, and easy industrialization, and opens up a new way for the resource utilization of kaolin.
[0068] Preferably, see Appendix Figure 2 In the step S100, the particle size of the kaolin after grinding is preferably 74 μm, the activation temperature is preferably 600° C., and the activation time is preferably 40 minutes.
[0069] 74 μm corresponds to a 200-mesh sieve. The present invention finds that under the above grinding particle size, activation temperature and activation time conditions, a better activation effect can be obtained, and the reaction speed of the subsequent acid leaching reaction can be further significantly improved.
[0070] Preferably, see Appendix Figure 2 In the step S200, the liquid-to-solid ratio of the first sulfuric acid solution to the sample M is preferably 10, the temperature condition is preferably 70° C., the concentration of the first sulfuric acid solution is preferably 1.5 mol / L, and the stirring dissolution time is preferably 60 min.
[0071] The above parameter conditions are an excellent parameter combination in the acid leaching reaction, which can further achieve the technical effect of leaching the aluminum, iron and gallium elements in the sample M into the solution faster and more fully, and the residual acid concentration in the solution after the reaction is low, thereby avoiding excessive acid and lime consumption in the subsequent steps during the pH adjustment process.
[0072] Preferably, in step S300, the adsorption resin is LX-92 resin, CL-P204 leaching resin, IRA900 resin, and / or chelating resin.
[0073] Preferably, in step S300, gallium ions are adsorbed by an adsorption resin at a temperature of 50° C., and after the resin adsorbing gallium is taken out, gallium sulfate is preferably eluted by a second sulfuric acid solution with a concentration of 3 mol / L at 60° C. for 20-60 minutes.
[0074] Through the above settings, the adsorption speed and elution adequacy of gallium element can be further improved, the waste of gallium element can be avoided as much as possible, and purer gallium sulfate can be obtained.
[0075] Preferably, see Appendix Figure 2 In the step S400, lime is preferably added to the filtrate B at 45° C., and the pH value of the filtrate is preferably controlled at 2.8.
[0076] The above parameter settings will help dissolve the lime as quickly as possible and will also facilitate the efficient precipitation of iron hydroxide and calcium sulfate.
[0077] Preferably, see Appendix Figure 2 In step S500, the concentration of the third sulfuric acid solution is preferably 3 mol / L, the liquid-to-solid ratio of the third sulfuric acid solution to the mixture of ferric hydroxide and calcium sulfate is preferably 4, the temperature condition is preferably 75° C., and the reaction time is preferably 15 minutes.
[0078] By setting the above parameters, the precipitation rate of iron hydroxide in step S400 and the dissolution rate of iron hydroxide in the third sulfuric acid solution in step S500 can be further improved, which helps to further improve the production efficiency of the kaolin resource utilization method of the present invention.
[0079] Preferably, see Appendix Figure 2 In the step S600, the calcination temperature is preferably 800° C., and the calcination time is preferably 40 minutes.
[0080] Preferably, see Appendix Figure 2 In the step S700, the calcination temperature is preferably 750° C., and the calcination time is preferably 40 minutes.
[0081] Through the above arrangement, the corresponding oxides (iron oxide and aluminum oxide) can be obtained efficiently, quickly and fully without causing excessive waste of heating resources.
[0082] Embodiment 1:
[0083] The kaolin in this embodiment has a SiO2 content of 39.6%, an Al2O3 content of 39.0%, a Fe2O3 content of 0.90%, and a Ga content of 76 μg / g. The specific steps of the kaolin full resource utilization method are as follows:
[0084] S100, kaolin was ground to a particle size of 74 μm and then activated at 600 °C for 40 min to obtain sample M;
[0085] S200, placing the sample M in a first sulfuric acid solution with a concentration of 1.5 mol / L at a temperature of 70°C according to a liquid-to-solid ratio of 10, stirring and dissolving for 60 minutes, and then filtering to obtain silicon micropowder and filtrate A;
[0086] S300, using LX-92 resin to adsorb gallium ions on filtrate A at 50°C, and the solution obtained after adsorbing gallium is filtrate B. After taking out the resin adsorbing gallium, eluting it with a 3 mol / L sulfuric acid solution at 40°C to obtain gallium sulfate;
[0087] S400, adding lime to the filtrate B at 50° C. to adjust the pH value of the filtrate B to 2.8, and monitoring the pH value of the filtrate B in real time, and when the pH value of the solution drops below 2.8, adding lime to return the pH value to 2.8, and when no lime needs to be added and the pH value does not drop below 2.8 for more than 20 minutes, filtering to obtain a mixture of ferric hydroxide and calcium sulfate and a filtrate C;
[0088] S500, dissolving the mixture of iron hydroxide and calcium sulfate obtained in step S400 in a third sulfuric acid solution with a concentration of 3 mol / L at a temperature of 70° C. at a liquid-to-solid ratio of 5, reacting for 20 minutes, and filtering to obtain calcium sulfate and filtrate D;
[0089] S600, the filtrate C is crystallized to obtain aluminum sulfate, which is calcined at 800°C for 40 minutes to obtain aluminum oxide and SO3, and the SO3 is recovered and returned to the process for acid production;
[0090] S700, the filtrate D is crystallized to obtain iron sulfate, which is calcined at 750° C. for 40 min to obtain iron oxide and SO3, and the SO3 is recovered and then returned to the above reaction step for use in acid production.
[0091] Embodiment 2:
[0092] The kaolin in this embodiment has a SiO2 content of 40.2%, an Al2O3 content of 39.8%, a Fe2O3 content of 0.86%, and a Ga content of 85 μg / g. The specific steps of the kaolin full resource utilization method are as follows:
[0093] S100, kaolin was ground to a particle size of 74 μm and then activated at 650 °C for 30 min to obtain sample M;
[0094] S200, placing the sample M in a first sulfuric acid solution with a concentration of 3 mol / L at a temperature of 80°C according to a liquid-to-solid ratio of 6, stirring and dissolving for 90 minutes, filtering, and obtaining silicon micropowder and filtrate A;
[0095] S300, using LX-92 resin to adsorb gallium ions on filtrate A at 60°C, and the solution obtained after adsorbing gallium is filtrate B. After the gallium adsorption is completed, the resin is taken out and eluted with a second sulfuric acid solution with a concentration of 2 mol / L at 60°C to obtain gallium sulfate;
[0096] S400, adding lime to the filtrate B at 50° C. to adjust the pH value of the filtrate B to 3.0, monitoring the pH value of the filtrate B in real time, adding lime to the filtrate B to return the pH value to 3.0 when the pH value of the solution drops below 3.0, and filtering to obtain a mixture of ferric hydroxide and calcium sulfate and a filtrate C when no lime needs to be added and the pH value does not drop below 3.0 for more than 20 minutes;
[0097] S500, dissolving the mixture of ferric hydroxide and calcium sulfate obtained in step S400 in a third sulfuric acid solution with a concentration of 4 mol / L at a temperature of 50° C. at a liquid-to-solid ratio of 7, reacting for 25 minutes, and filtering to obtain calcium sulfate and filtrate D;
[0098] S600, the filtrate C is crystallized to obtain aluminum sulfate, which is calcined at 750° C. for 60 min to obtain aluminum oxide and SO3, and the SO3 is recovered to make acid and then returned to the above reaction step for use;
[0099] S700, the filtrate D is crystallized to obtain iron sulfate, which is calcined at 750° C. for 40 min to obtain iron oxide and SO3, and the SO3 is recovered and then returned to the above reaction step for use in acid production.
[0100] Those skilled in the art will appreciate that, without conflict, the above-mentioned preferred solutions can be freely combined and superimposed.
[0101] It should be understood that the above-mentioned embodiments are merely illustrative and not restrictive. Without departing from the basic principles of the present invention, various obvious or equivalent modifications or substitutions that can be made by those skilled in the art to the above-mentioned details will all be included in the scope of the claims of the present invention.
Claims
1. A method for fully utilizing kaolin resources, It is characterized in that The following steps are involved: S100, grinding kaolin to a particle size of 50-90 μm, activating at a temperature of 200-700° C. for 30-60 min, and obtaining sample M; S200, placing the sample M in a first sulfuric acid solution with a concentration of 1 to 6 mol / L at a temperature of 40 to 90° C. at a liquid-to-solid ratio of 4 to 10, stirring and dissolving for 30 to 90 minutes, and then filtering to obtain silicon micropowder and filtrate A; S300, adsorbing gallium ions with an adsorption resin at a temperature of 40 to 60° C. on the filtrate A, and obtaining a solution after adsorbing gallium as the filtrate B. After the gallium adsorption is completed, the resin is taken out, and eluted with a second sulfuric acid solution with a concentration of 2 to 3 mol / L at a temperature of 40 to 60° C. to obtain gallium sulfate; S400, adding lime to the filtrate B at 40-60° C. to adjust the pH value of the filtrate B to between 2.5 and 3.3, monitoring the pH value of the filtrate B in real time, and when the pH value of the solution drops below 2.5, adding lime to return the pH value to 2.5-3.3, and filtering when no lime needs to be added and the pH value does not drop below 2.5 for more than 20 minutes, to obtain a mixture of ferric hydroxide and calcium sulfate and a filtrate C; S500, dissolving the mixture of ferric hydroxide and calcium sulfate obtained in step S400 in a third sulfuric acid solution having a concentration of 2 to 4 mol / L at a temperature of 40 to 90° C. at a liquid-to-solid ratio of 3 to 7, reacting for 5 to 30 minutes, and filtering to obtain calcium sulfate and filtrate D; S600, the filtrate C is crystallized to obtain aluminum sulfate, which is calcined at 750-850°C for 20-60 min to obtain aluminum oxide and SO 3 , to SO 3 After the acid is recovered, it is returned to the aforementioned reaction step for use; S700, the filtrate D is crystallized to obtain iron sulfate, which is calcined at 700-800°C for 20-60min to obtain iron oxide and SO 3 , SO 3 The acid is recovered and returned to the above reaction step for use.
2. The method according to claim 1, It is characterized in that In the step S100, the particle size of the kaolin after grinding is preferably 74 μm, the activation temperature is preferably 600° C., and the activation time is preferably 40 minutes.
3. The method according to claim 1, It is characterized in that In the step S200, the liquid-to-solid ratio of the first sulfuric acid solution to the sample M is preferably 10, the temperature condition is preferably 70°C, the concentration of the first sulfuric acid solution is preferably 1.5 mol / L, and the stirring dissolution time is preferably 60 min.
4. The method according to claim 1, It is characterized in that In the step S300, the adsorption resin is LX-92 resin, CL-P204 leaching resin, IRA900 resin, and / or chelating resin.
5. The method according to claim 1, It is characterized in that In the step S300, gallium ions are preferably adsorbed by an adsorption resin at a temperature of 50°C. After the resin adsorbing gallium is taken out, gallium sulfate is preferably eluted with a second sulfuric acid solution with a concentration of 3 mol / L at 60°C for 20 to 60 minutes.
6. The method according to claim 1, It is characterized in that In the step S400, lime is preferably added to the filtrate B at 45°C, and the pH value of the filtrate is preferably controlled at 2.
8.
7. The method according to claim 1, It is characterized in that In the step S500, the concentration of the third sulfuric acid solution is preferably 3 mol / L, the liquid-to-solid ratio of the third sulfuric acid solution to the mixture of ferric hydroxide and calcium sulfate is preferably 4, the temperature condition is preferably 75° C., and the reaction time is preferably 15 min.
8. The method according to claim 1, It is characterized in that In the step S600, the calcination temperature is preferably 800°C, and the calcination time is preferably 40 minutes.
9. The method according to claim 1, It is characterized in that In the step S700, the calcination temperature is preferably 750°C, and the calcination time is preferably 40 minutes.
Citation Information
Patent Citations
Method for preparing ultra-fine white carbon black and nano alumina by using kaolinite as raw material
CN101249965A
Comprehensive utilization method of vanadium slag in metal gallium production process
CN114507778A
Comprehensive utilization method of red mud
CN117003290A
Aolinite
KR1020000040938A
Method for stepwise extraction of silica and hydroxide from silicate substances
US20220267159A1