Method for harmlessly treating bottom mud of aquaculture pond through low-temperature aerobic pyrolysis and producing spray-dried carrier particles

The aquaculture pond sediment is processed through twin-screw squeezing and low-temperature aerobic pyrolysis technology to form calcium-carbon-based particles with a mesoporous structure, which solves the problem of dehydration and harmlessness of high-moisture content sediment and is suitable for spray drying carriers , and reduce energy consumption and raw material costs.

CN118851522AActive Publication Date: 2024-10-29NANJING UNIV +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410906042.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-29
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

The existing technology is difficult to efficiently dehydrate and harmlessly treat aquaculture pond sediments with high moisture content, and it is difficult to form particles with mesoporous pores and large specific surface areas suitable as spray drying carriers.

Method used

Using twin-screw extrusion and granulation integrated equipment and a low-temperature aerobic pyrolysis rotary reactor, through the combination of carbide slag and straw powder, low-temperature aerobic pyrolysis of the bottom sludge is achieved to form calcium-carbon-based particles with a mesoporous structure. For spray drying carriers.

Benefits of technology

It achieves efficient dehydration and harmless treatment of bottom sludge, forming calcium-carbon-based particles with larger mesopore diameter and specific surface area, which are suitable for spray drying carriers, reduce energy consumption, and achieve resource utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004932127170000011
    Figure HDA0004932127170000011
Patent Text Reader

Abstract

The invention discloses a method for harmlessness and production of spray-dried carrier particles by low-temperature aerobic pyrolysis of bottom mud of an aquaculture pond. The bottom mud of the aquaculture pond, the carbide slag and the straw powder are combined, the bottom mud and the straw are pyrolyzed in the low-temperature aerobic pyrolysis process to form a good mesoporous space structure, and calcium carbonate is generated through the reaction of the carbide slag, the atmosphere and carbon dioxide generated through pyrolysis to directly provide the particle strength; and finally, calcium-carbon-based particles with certain particle strength and a good mesoporous space system are formed and can be used for spray drying of a carrier.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of low-temperature aerobic pyrolysis and resource utilization of aquaculture pond sludge in environmental engineering, and specifically relates to a method for harmless low-temperature aerobic pyrolysis of aquaculture pond sludge and production of spray-dried carrier particles. Background Art

[0002] The bottom mud of aquaculture ponds is composed of a large amount of minerals and organic matter (uneaten bait residues, antibiotics, excrement, and organic matter after the death of various organisms), and is an important carrier for the accumulation, migration and transformation of pollutants. Too thick bottom mud will form a local anaerobic environment at the bottom of the pond, forming a large number of products that are toxic to aquaculture organisms (such as ammonia, hydrogen sulfide, organic acids, etc.). At the same time, the complex bottom mud is also easy to breed pathogens, and the accumulated antibiotics induce pathogens to form antibiotic resistance genes, resulting in frequent diseases of aquaculture organisms, which seriously affects the quality and health safety of aquaculture products.

[0003] In large-scale agricultural aquaculture, due to high-density breeding and large amounts of feeding, pond sediments are prone to accumulation and deposition, so they need to be properly treated and disposed of. After two to three years of aquaculture ponds, the sediments need to be treated by pond cleaning, that is, after the ponds are exposed to the sun, part of the sediment is dug out and placed on the pond bank, and the bottom of the pond is disinfected with quicklime to eliminate parasites, pathogens and other harmful organisms in the sediment. Although placing the sediment on the pond bank greatly reduces the treatment cost and saves manpower and material resources, the hydraulic effects such as rainwater erosion will still cause organic matter, antibiotics and other pollutants in the sediment to migrate to the breeding pond, making pond cleaning insufficient. At present, the main ex situ treatment and disposal technologies for pond sediments in my country include aerobic composting, anaerobic digestion, and pyrolysis technology. Among them, pyrolysis technology has broad application prospects due to its good environmental and economic benefits, but due to the high water content of the sediment, more inorganic matter, and difficulty in pyrolysis, it is often mixed with pyrolysis by adding biomass such as straw and garden waste.

[0004] Chinese patent CN113171750B discloses a method for preparing biochar using sludge and garden waste, the method comprising drying and crushing the sludge and garden waste, adding water at a mass ratio of 1:0.25-4 to mix evenly, and pyrolyzing at 300-700°C for 1-5h in anoxic conditions, and mixing the pyrolysis product with a modifier (NaOH or FeCl3) with water evenly, and drying to obtain the final product, biochar. Although this method can effectively treat sludge and garden waste by pyrolysis and convert them into biochar, it undergoes multiple drying and anoxic processes, has high energy consumption, and also requires the addition of modifiers, resulting in high raw material costs, and is not suitable for large-scale aquaculture sludge treatment and disposal.

[0005] Chinese patent CN115477527B discloses a method for producing biochar ceramsite particle filler, which mixes sludge with industrial waste such as fly ash, and uses a low-temperature aerobic pyrolysis process to render the sludge harmless and form biochar ceramsite with a spatial porous structure, which can be used for the adsorption of gas-liquid multi-media pollutants. However, the average mesopore diameter of the biochar ceramsite is 6-10nm, which is relatively small and is not suitable as a spray drying carrier.

[0006] Therefore, how to further achieve efficient dehydration and harmlessness of high-water content sludge, reduce process energy consumption, and utilize sludge pyrolysis to form spray-dried carrier particles with larger mesoporous pores and specific surface area are issues that need to be urgently addressed. Summary of the invention

[0007] The problems that need to be solved in the above-mentioned prior art are as follows: (1) efficient dehydration and harmlessness of high-water content sludge; (2) using sludge pyrolysis to form carrier particles with larger mesoporous pores and specific surface area as carriers for spray drying.

[0008] The present invention provides a method for harmless treatment of bottom mud in aquaculture ponds by low-temperature aerobic pyrolysis and production of spray-dried carrier particles. The method realizes efficient dehydration of bottom mud with high water content and harmless treatment by low-temperature aerobic pyrolysis by using a twin-screw extrusion granulation integrated device and a low-temperature aerobic pyrolysis rotary reactor; and by adding carbide slag and crushed straw powder, the bottom mud can form relatively large mesoporous pores (mesopore diameter is about 23nm) by low-temperature aerobic pyrolysis of the bottom mud, and the mesoporous pore diameter can be improved by low-temperature aerobic pyrolysis of the straw powder and the specific surface area of ​​the calcium carbon-based particles can be increased (for example, the specific surface area of ​​the calcium carbon-based particles prepared after adding straw in Example 1 is 13.6764m 2 / g, and no straw was added to Example 1 for comparison, the specific surface area of ​​the prepared calcium carbon-based particles was 8.0947m 2 / g,); carbide slag can react with the atmosphere and pyrolysis to produce carbon dioxide to generate calcium carbonate, which directly provides particle strength. Finally, calcium carbon-based particles with a certain particle strength and a mesoporous spatial structure are obtained through low-temperature aerobic pyrolysis. The good mesoporous system can be used as a carrier for spray drying.

[0009] The technical solution adopted by the present invention is as follows:

[0010] A method for harmless treatment of aquaculture pond sludge by low-temperature aerobic pyrolysis and production of spray-dried carrier particles, the method comprising the following steps:

[0011] Step 1): mixing aquaculture pond sludge, carbide slag and straw powder;

[0012] Step 2): the mixed material is squeezed and dehydrated in a twin-screw extrusion and granulation integrated equipment and pressure-formed to form wet-based columnar particles;

[0013] Step 3): The wet columnar particles are sent to a low-temperature aerobic pyrolysis rotary reactor, and the bottom mud of aquaculture ponds is rendered harmless through particle preheating, low-temperature aerobic pyrolysis and instantaneous combustion. Calcium carbon-based particles with particle strength and a mesoporous spatial structure are obtained. The calcium carbon-based particles with a good mesoporous system can be used as spray drying carriers.

[0014] Furthermore, in step 1), the bottom mud of aquaculture pond comes from the process of cleaning or maintaining aquaculture pond, and has a water content of 90-95%; carbide slag is the main industrial waste of electrolytic acetylene production, and its main component is calcium hydroxide; the straw is crushed into straw powder with a size of 10-20 mesh.

[0015] Furthermore, in step 1), the mass ratio of the materials to be stirred and mixed is 5-6:2:2-3 for the bottom mud:carbide slag:straw powder;

[0016] Aquaculture pond sludge, carbide slag and straw powder are respectively transported to the mixer through shaftless screws;

[0017] The moisture content of the material after stirring and mixing is 55-70%.

[0018] Furthermore, in step 2), the mixed material is conveyed to a twin-screw extrusion and granulation integrated device through a shaftless screw; the twin-screw extrusion and granulation integrated device is a sludge mixed material pressure molding granulation moisture content control device disclosed in Chinese patent CN 117839550 A.

[0019] Furthermore, in step 2), the mixed material is first dehydrated by twin-screw extrusion and friction evaporation, and the moisture content of the mixed material is controlled to be 25-32% to achieve continuous and stable granulation. The dehydration is completed in the moisture control section of the sludge mixed material pressure molding granulation moisture content control equipment;

[0020] The mixed material is then pressure-formed to form wet-based columnar particles with a diameter of 3 to 10 mm and a length of 5 to 10 mm, and the moisture content of the wet-based columnar particles is 20 to 25%. Granulation is completed in the extrusion granulation section of the sludge mixed material pressure-forming granulation moisture content control equipment.

[0021] Further, in step 3): during the low-temperature aerobic pyrolysis process, the drug residues in the sludge, the organic matter of fish feces and the biomass of the straw are carbonized and rendered harmless, and a multi-mesoporous spatial structure is formed inside the columnar particles; at the same time, the carbon dioxide produced by pyrolysis and the carbon dioxide in the atmosphere react with the carbide slag to form calcium carbonate, providing particle strength for the columnar particles, and finally forming calcium-carbon-based particles with particle strength and a good mesoporous system, which can be used as a spray drying carrier. The low-temperature aerobic pyrolysis rotary reactor is the horizontal rotary aerobic pyrolysis furnace described in CN115477527B.

[0022] Furthermore, in step 3), the particle preheating temperature is 100-150° C., and the moisture content of the wet-based columnar particles after preheating is reduced to 15-20%; the temperature of low-temperature aerobic pyrolysis is 350-375° C., and the residence time is 20-30 minutes; the temperature of instantaneous combustion is 1000-1200° C., and the residence time is 5-15 seconds.

[0023] Furthermore, the low-temperature aerobic pyrolysis: it is necessary to determine the required oxygen and carbon dioxide content according to the calcium hydroxide content in the carbide slag and the amount of oxygen required for the low-temperature aerobic pyrolysis of the sludge and straw organic matter, that is, to determine the addition ratio of air and industrial flue gas, and monitor the exhaust gas oxygen and carbon dioxide concentrations in the intake air in real time through the gas concentration probe at the air inlet at the front end of the reactor; at the same time, it is necessary to set a gas concentration probe at the air outlet at the rear end of the reactor to monitor the exhaust gas oxygen and carbon dioxide concentrations in real time, and adjust the intake air and industrial flue gas ratio based on the circulating exhaust gas ratio.

[0024] Furthermore, in step 3), the exhaust gas is cooled by a heat exchanger and the incoming air is preheated at the same time. After the exhaust gas is cooled, it is passed through a humus fixed bed to remove pollutant components in the gas, and is discharged into the air after being determined to meet the standards.

[0025] Compared with the prior art, the beneficial effects of the present invention are:

[0026] (1) The present invention solves the problem of dehydration of aquaculture pond sludge by twin-screw squeezing technology, and realizes the carbonization and harmlessness of drug residues, organic matter such as fish feces, and straw biomass in the aquaculture pond sludge by low-temperature aerobic pyrolysis technology. The present invention has low energy consumption, simple and flexible operation, and little impact on the environment.

[0027] (2) The present invention combines aquaculture pond sludge, carbide slag and straw powder, and forms a good mesoporous (average pore size is 20nm) spatial structure through low-temperature aerobic pyrolysis of the sludge and straw (the average mesopore size formed by low-temperature aerobic pyrolysis of the sludge is relatively large, about 23nm; the straw has a high organic matter content, and aerobic pyrolysis can further improve the pore structure and specific surface area of ​​the calcium carbon-based particles). Calcium carbonate is generated by the reaction of carbide slag with the atmosphere and carbon dioxide produced by pyrolysis to directly provide particle strength, and finally calcium carbon-based mesoporous particles with a certain particle strength and a good mesoporous system are formed, which can be used as a spray drying carrier.

[0028] (3) The present invention produces spray-dried carrier particles by low-temperature aerobic pyrolysis in an atmosphere of CO2 from industrial flue gas and O2 from air, organically combining aerobic pyrolysis of aquaculture pond sludge and straw biomass with CO2 fixation in industrial flue gas, thereby achieving harmlessness of aquaculture pond sludge through low-temperature aerobic pyrolysis, carbon emission reduction through CO2 fixation in industrial flue gas, and resource utilization of the output of spray-dried carrier particles.

[0029] (4) The present invention utilizes high-water content biomass waste (aquaculture pond mud), industrial waste (carbide slag) and farmland waste (straw) to produce spray-dried carrier particles. The raw materials are easily available, low-cost, simple and practical, and the plant construction conditions are simple and flexible, with less equipment investment, less secondary pollution, and little impact on the environment. It has good economic and environmental benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The present invention is a process flow chart of the method for low-temperature aerobic pyrolysis of aquaculture pond sludge to render it harmless and for producing spray-dried carrier particles. DETAILED DESCRIPTION

[0031] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the technical solutions in the embodiments of the present invention are clearly and completely described below in conjunction with the accompanying drawings.

[0032] The method of low-temperature aerobic pyrolysis and harmless treatment of aquaculture pond sludge and production of spray-dried carrier particles in this embodiment includes the following:

[0033] Step 1): stirring and mixing aquaculture sludge, carbide slag and straw powder;

[0034] Furthermore, the aquaculture pond sludge comes from the aquaculture pond cleaning or maintenance process, and has a water content of 90-95%; carbide slag is the main industrial waste from electrolysis to produce acetylene, and its main component is calcium hydroxide; the straw is crushed to a size of 10-20 meshes.

[0035] Preferably, in step 1), the material ratio of the mixed material is 6:2:2 or 5:2:3 of sludge: carbide slag: straw; the materials are respectively transported to the mixer through a shaftless screw; the moisture content of the material after stirring and mixing is 55%-70%.

[0036] Step 2): the mixed material is squeezed and dehydrated in a twin-screw squeeze and granulation integrated device and pressure-formed to form wet-based columnar particles with a certain particle strength;

[0037] Preferably, in the step 2), the mixed material is conveyed to the twin-screw extrusion granulation integrated equipment by a shaftless screw, the material is first dehydrated by twin-screw extrusion and friction evaporation, and the moisture content of the mixed material is controlled to 25%-32% by controlling the operating parameters such as the twin-screw speed to achieve continuous and stable granulation;

[0038] Preferably, the mixed material with suitable moisture content in step 2) enters the pressure forming section of the twin-screw extrusion granulation integrated equipment to form wet-based columnar particles with a diameter of 3-10 mm and a length of 5-10 mm through pressure forming, and the moisture content of the wet-based columnar particles is 20%-25%.

[0039] Step 3): The wet-based particles are sent to a low-temperature aerobic pyrolysis rotary reactor, and are subjected to particle preheating, low-temperature aerobic pyrolysis and instantaneous combustion treatment to obtain calcium carbon-based mesoporous particles with a certain particle strength. The good mesoporous system can be used as a spray drying carrier.

[0040] Preferably, in the step 3), the temperature of the preheating section of the low-temperature aerobic pyrolysis rotary reactor is 100-150°C, and the moisture content of the wet-based columnar particles after preheating is reduced to 15%-20%; the temperature of the low-temperature aerobic pyrolysis section is 350-375°C, and the residence time is 20-30min; the temperature of the instantaneous combustion is 1000-1200°C, and the residence time is 5-15s.

[0041] Preferably, in the step 3), the low-temperature aerobic pyrolysis section of the low-temperature aerobic pyrolysis rotary reactor needs to determine the ratio of air and industrial flue gas addition according to the carbide slag content and the oxygen demand of the low-temperature aerobic pyrolysis, and monitor it in real time through the gas concentration probe at the air inlet at the front end of the reactor; at the same time, a gas concentration probe needs to be set at the air outlet at the rear end of the reactor to monitor the oxygen and carbon dioxide concentrations of the exhaust gas in real time, and adjust the ratio of intake air and industrial flue gas based on the circulating exhaust gas ratio.

[0042] Preferably, in step 3), the exhaust gas is cooled by a heat exchanger and the incoming air is preheated at the same time. After the exhaust gas is cooled, it passes through a humus fixed bed to remove pollutant components in the gas, and is discharged into the air after being determined to meet the standards.

[0043] During the low-temperature aerobic pyrolysis process, drug residues, organic matter such as fish feces, sludge organic matter, and straw biomass in the bottom mud are carbonized and rendered harmless, and a multi-mesoporous space structure is formed inside the columnar particles. At the same time, the carbon dioxide produced by pyrolysis and the carbon dioxide in the atmosphere react with carbide slag to form calcium carbonate, which provides particle strength for the columnar particles, and finally forms calcium-carbon-based particles with a certain particle strength and a good mesoporous system, which can be used as spray drying carriers.

[0044] Embodiment 1:

[0045] (1): Aquaculture sludge (water content of 90%), carbide slag and straw powder (crushed to 15 meshes) are respectively transported to a horizontal mixer through a shaftless screw at a ratio of sludge: carbide slag: straw of 6:2:2 for stirring and mixing;

[0046] (2): The mixed material is conveyed to the twin-screw extrusion granulation integrated equipment through a shaftless screw. The material is first dehydrated under the action of twin-screw extrusion and friction evaporation. By controlling the operating parameters such as the twin-screw speed, the moisture content of the mixed material is controlled to drop from 60% to 28%-32% to achieve continuous and stable granulation; the mixed material with an appropriate moisture content enters the pressure forming section of the twin-screw extrusion granulation integrated equipment and is pressure-formed to form wet-based columnar particles with a diameter of 8 mm and a length of 10 mm. The moisture content of the wet-based columnar particles is 25%.

[0047] (3): The wet-based particles are sent to a low-temperature aerobic pyrolysis rotary reactor. The temperature of the preheating section of the low-temperature aerobic pyrolysis rotary reactor is 125°C. After preheating, the moisture content of the wet-based columnar particles is reduced to 20%; the temperature of the low-temperature aerobic pyrolysis section is 375°C, and the residence time is 30 minutes; the temperature of the instantaneous combustion is 1100°C, and the residence time is 10 seconds. The proportion of air and industrial flue gas added is determined according to the carbide slag content and the oxygen demand of low-temperature aerobic pyrolysis, and the gas concentration probes at the front air inlet and outlet of the reactor are used for real-time monitoring and the proportion of intake air and industrial flue gas added is adjusted based on the proportion of circulating tail gas.

[0048] (4) When the exhaust gas is discharged, it is cooled by heat exchanger and the incoming air is preheated at the same time. After the exhaust gas is cooled, it passes through a humus fixed bed to remove pollutants in the gas. After being tested and found to meet the standards, it is discharged into the air.

[0049] During the low-temperature aerobic pyrolysis process, drug residues, organic matter such as fish feces, sludge organic matter, and straw biomass in the bottom mud are carbonized and rendered harmless, and a multi-mesoporous space structure is formed inside the columnar particles. At the same time, the carbon dioxide produced by pyrolysis and the carbon dioxide in the atmosphere react with carbide slag to form calcium carbonate, which provides particle strength for the columnar particles. Finally, calcium-carbon-based particles with a certain particle strength and a good mesoporous system are obtained, which can be used as spray drying carriers.

[0050] The mesoporous calcium carbon-based particles prepared in this example have a compressive strength of 100.35N and a BET specific surface area of ​​13.6764m 2 / g, total pore volume: 0.062519cm 3 / g, average pore size: 18.2854nm.

[0051] Embodiment 2:

[0052] (1): Aquaculture sludge (water content of 92%), carbide slag and straw powder (crushed to 10 meshes) are respectively transported to a horizontal mixer through a shaftless screw at a ratio of sludge: carbide slag: straw of 5:2:3 for stirring and mixing;

[0053] (2): The mixed material is conveyed to the twin-screw extrusion granulation integrated equipment through a shaftless screw. The material is first dehydrated under the action of twin-screw extrusion and friction evaporation. By controlling the operating parameters such as the twin-screw speed, the moisture content of the mixed material is controlled to decrease from 55% to 30% to achieve continuous and stable granulation; the mixed material with an appropriate moisture content enters the pressure forming section of the twin-screw extrusion granulation integrated equipment and is pressure-formed to form wet-based columnar particles with a diameter of 5 mm and a length of 7 mm. The moisture content of the wet-based columnar particles is 25%.

[0054] (3): The wet-based particles are sent to a low-temperature aerobic pyrolysis rotary reactor. The temperature of the preheating section of the low-temperature aerobic pyrolysis rotary reactor is 150°C. After preheating, the moisture content of the wet-based columnar particles drops to 18%; the temperature of the low-temperature aerobic pyrolysis section is 365°C, and the residence time is 25 minutes; the temperature of the instantaneous combustion is 1200°C, and the residence time is 15 seconds. The proportion of air and industrial flue gas added is determined based on the carbide slag content and the oxygen demand of low-temperature aerobic pyrolysis, and the gas concentration probes at the front air inlet and outlet of the reactor are used for real-time monitoring and the proportion of intake air and industrial flue gas added is adjusted based on the proportion of circulating tail gas.

[0055] (4) When the exhaust gas is discharged, it is cooled by heat exchanger and the incoming air is preheated at the same time. After the exhaust gas is cooled, it passes through a humus fixed bed to remove pollutants in the gas. After being tested and found to meet the standards, it is discharged into the air.

[0056] During the low-temperature aerobic pyrolysis process, drug residues, organic matter such as fish feces, sludge organic matter, and straw biomass in the bottom mud are carbonized and rendered harmless, and a multi-mesoporous space structure is formed inside the columnar particles. At the same time, the carbon dioxide produced by pyrolysis and the carbon dioxide in the atmosphere react with carbide slag to form calcium carbonate, which provides particle strength for the columnar particles. Finally, calcium-carbon-based particles with a certain particle strength and a good mesoporous system are obtained, which can be used as spray drying carriers.

[0057] The mesoporous calcium carbon-based particles prepared in this example have a compressive strength of 120.35N and a BET specific surface area of ​​14.7327m 2 / g, total pore volume: 0.069541cm 3 / g, average pore size: 19.3815nm.

[0058] Embodiment 3:

[0059] (1): Aquaculture sludge (water content of 90%), carbide slag and straw powder (crushed to 12 meshes) are respectively transported to a horizontal mixer through a shaftless screw at a ratio of sludge: carbide slag: straw of 5:2:3 for stirring and mixing;

[0060] (2): The mixed material is conveyed to the twin-screw extrusion granulation integrated equipment through a shaftless screw. The material is first dehydrated under the action of twin-screw extrusion and friction evaporation. By controlling the operating parameters such as the twin-screw speed, the moisture content of the mixed material is controlled to drop from 58% to 28% to achieve continuous and stable granulation; the mixed material with an appropriate moisture content enters the pressure forming section of the twin-screw extrusion granulation integrated equipment and is pressure-formed to form wet-based columnar particles with a diameter of 3 mm and a length of 5 mm. The moisture content of the wet-based columnar particles is 23%.

[0061] (3): The wet-based particles are sent to a low-temperature aerobic pyrolysis rotary reactor. The temperature of the preheating section of the low-temperature aerobic pyrolysis rotary reactor is 100°C. After preheating, the moisture content of the wet-based columnar particles is reduced to 20%; the temperature of the low-temperature aerobic pyrolysis section is 370°C, and the residence time is 28 minutes; the temperature of the instantaneous combustion is 1150°C, and the residence time is 12 seconds. The proportion of air and industrial flue gas added is determined according to the carbide slag content and the oxygen demand of low-temperature aerobic pyrolysis, and the gas concentration probes at the front air inlet and outlet of the reactor are used for real-time monitoring and the proportion of intake air and industrial flue gas added is adjusted based on the proportion of circulating tail gas.

[0062] (4) When the exhaust gas is discharged, it is cooled by heat exchanger and the incoming air is preheated at the same time. After the exhaust gas is cooled, it passes through a humus fixed bed to remove pollutants in the gas. After being tested and found to meet the standards, it is discharged into the air.

[0063] During the low-temperature aerobic pyrolysis process, drug residues, organic matter such as fish feces, sludge organic matter, and straw biomass in the bottom mud are carbonized and rendered harmless, and a multi-mesoporous space structure is formed inside the columnar particles. At the same time, the carbon dioxide produced by pyrolysis and the carbon dioxide in the atmosphere react with carbide slag to form calcium carbonate, which provides particle strength for the columnar particles. Finally, calcium-carbon-based particles with a certain particle strength and a good mesoporous system are obtained, which can be used as spray drying carriers.

[0064] The mesoporous calcium carbon-based particles prepared in this example have a compressive strength of 99.73N and a BET specific surface area of ​​14.3073m 2 / g, total pore volume: 0.066732cm 3 / g, average pore size: 20.8819nm.

[0065] Comparative Example 1:

[0066] According to the Chinese patent CN115477527B, Example 1 of a method for producing biochar ceramsite particle filler is prepared as follows:

[0067] A small amount of lime is added to the dehydrated cake of biomass waste with a moisture content of 80%, and heated and stirred at 60°C for pretreatment; the pretreated material is placed in a plate and frame filter press to further reduce the moisture content of the material to 50% as the main material, accounting for 50%, and fly ash, phosphogypsum and lime are prepared in a mass ratio of about 8:1:1, and the waste plastic residue is crushed to less than 2mm, and added to the intermittently running horizontal mixing tank by screw conveyor according to the mass ratio of 6% of the main and auxiliary mixed materials to fully mix; the mixed material is evenly fed into the inlet of the twin-screw extruder, the extruder die head adopts a 5mm orifice plate and is equipped with an automatic scraper, and the mixed material is processed by pressure molding into wet-based columnar particles with a diameter of 5mm and a length of 5-10mm (moisture content 30-40%); the wet-based column The wet-based columnar particles are sent to the entrance of the horizontal rotary aerobic pyrolysis furnace by a belt conveyor. The temperature of the wet-based columnar particles is raised to 150°C through the waste heat exhaust preheating and drying section, and the moisture content is reduced to 25%; then they enter the low-temperature aerobic pyrolysis section, the temperature is gradually raised to 300°C, and the particles slowly rotate and stay for 40 minutes; the particles finally enter the instantaneous combustion section, at 250-350°C, using natural gas or other combustible gases as fuel, and the annular porous burner technology, at 250-350°C, the particles are subjected to short-term combustion treatment to burn out liquid phase products; finally, the dry-based particle products are discharged from the outlet of the pyrolysis furnace and are air-cooled; the dry-based particles are humidified by water mist and controlled at 50°C by electric heating in the wet curing tank for 5 days to obtain an environmentally friendly material biochar ceramsite product with good mechanical strength.

[0068] Finally, the biochar ceramsite particle filler with certain mechanical strength is obtained. The apparent density of biochar ceramsite is 1.097g / cm 3 , adsorption capacity: 12.26mg / g, compressive strength: 16.76N, BET surface area: 13.9053m 2 / g, total pore volume: 0.028698cm 3 / g, mesopore volume: 0.027715cm 3 / g, average pore size: 8.2552nm (mainly mesopores).

[0069] It can be seen that the average pore size of the biochar ceramsite prepared by Comparative Example 1 is small (8.2552 nm) and the compressive strength is poor.

[0070] The molecular weight of organic matter in liquid fertilizer concentrate is relatively large. If the pore size of the spray drying carrier is small, it will be detrimental to the mass transfer process of organic matter during the spray drying process. The average mesoporous pore size of the bottom mud-based calcium carbon-based particles of the present invention is higher than that of the biochar ceramsite in Comparative Example 1, which is beneficial as spray drying carrier particles for liquid fertilizer concentrate.

[0071] The above description is only a preferred embodiment of the present invention and does not constitute a limitation on the protection scope of the present invention. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention shall be included in the protection scope of the claims of the present invention.

Claims

1. A method for detoxifying aquaculture pond sludge by low-temperature aerobic pyrolysis and producing spray-dried carrier particles, characterized in that: The method comprises the following: Step 1): mixing aquaculture pond sludge, carbide slag and straw powder; Step 2): the mixed material is squeezed and dehydrated in a twin-screw extrusion and granulation integrated equipment and pressure-formed to form wet-based columnar particles; Step 3): The wet columnar particles are sent to a low-temperature aerobic pyrolysis rotary reactor, and the bottom mud of aquaculture ponds is rendered harmless through particle preheating, low-temperature aerobic pyrolysis and instantaneous combustion. Calcium carbon-based particles with particle strength and a mesoporous spatial structure are obtained. The calcium carbon-based particles with a good mesoporous system can be used as spray drying carriers.

2. The method for low-temperature aerobic pyrolysis of aquaculture pond sludge to detoxify and produce spray-dried carrier particles according to claim 1, characterized in that: In the step 1), the bottom mud of the aquaculture pond comes from the process of cleaning or maintaining the aquaculture pond, and has a water content of 90-95%; the carbide slag is the main industrial waste of electrolytic acetylene production, and its main component is calcium hydroxide; the straw is crushed into straw powder with a size of 10-20 mesh.

3. The method for low-temperature aerobic pyrolysis of aquaculture pond sludge to detoxify and produce spray-dried carrier particles as claimed in claim 2, characterized in that: The step 1): the mass ratio of the materials stirred and mixed is 5-6:2:2-3 for the bottom mud:carbide slag:straw powder; Aquaculture pond sludge, carbide slag and straw powder are respectively transported to the mixer through shaftless screws; The moisture content of the material after stirring and mixing is 55-70%.

4. The method for detoxifying aquaculture pond sludge by low-temperature aerobic pyrolysis and producing spray-dried carrier particles according to any one of claims 1 to 3, characterized in that: In the step 2), the mixed material is conveyed to the twin-screw extrusion and granulation integrated equipment through a shaftless screw; the twin-screw extrusion and granulation integrated equipment is a sludge mixed material pressure molding granulation moisture content control equipment in Chinese patent CN 117839550A.

5. The method for low-temperature aerobic pyrolysis of aquaculture pond sludge to detoxify and produce spray-dried carrier particles as claimed in claim 4, characterized in that: The step 2): the mixed material is first dehydrated by twin-screw extrusion and friction evaporation, and the moisture content of the mixed material is controlled to be 25-32% to achieve continuous and stable granulation; The mixed material is then formed into wet-based columnar particles with a diameter of 3 to 10 mm and a length of 5 to 10 mm by pressure molding, and the moisture content of the wet-based columnar particles is 20 to 25%.

6. The method for detoxifying aquaculture pond sludge by low-temperature aerobic pyrolysis and producing spray-dried carrier particles according to any one of claims 1 to 3, characterized in that: The step 3): during the low-temperature aerobic pyrolysis process, the drug residues in the sludge, the organic matter in fish feces and the biomass of the straw are carbonized and rendered harmless, and a multi-mesoporous space structure is formed inside the columnar particles; at the same time, the carbon dioxide generated by pyrolysis and the carbon dioxide in the atmosphere react with the carbide slag to form calcium carbonate, which provides particle strength for the columnar particles, and finally forms calcium-carbon-based particles with particle strength and a good mesoporous system, which can be used as a spray drying carrier.

7. The method for low-temperature aerobic pyrolysis of aquaculture pond sludge to detoxify and produce spray-dried carrier particles as claimed in claim 6, characterized in that: In the step 3), the particle preheating temperature is 100-150° C., and the moisture content of the wet-based columnar particles after preheating is reduced to 15-20%; the temperature of low-temperature aerobic pyrolysis is 350-375° C., and the residence time is 20-30 minutes; the temperature of instantaneous combustion is 1000-1200° C., and the residence time is 5-15 seconds.

8. The method for low-temperature aerobic pyrolysis of aquaculture pond sludge to detoxify and produce spray-dried carrier particles as claimed in claim 6, characterized in that: The low-temperature aerobic pyrolysis: the required oxygen and carbon dioxide content needs to be determined according to the calcium hydroxide content in the carbide slag and the amount of oxygen required for the low-temperature aerobic pyrolysis of the sludge and straw organic matter, that is, the addition ratio of air and industrial flue gas is determined, and the concentrations of exhaust oxygen and carbon dioxide in the intake air are monitored in real time through the gas concentration probe at the air inlet at the front end of the reactor; at the same time, a gas concentration probe needs to be set at the air outlet at the rear end of the reactor to monitor the concentrations of exhaust oxygen and carbon dioxide in real time, and the ratio of intake air and industrial flue gas is adjusted based on the circulating exhaust gas ratio.

9. The method for low-temperature aerobic pyrolysis of aquaculture pond sludge to detoxify and produce spray-dried carrier particles as claimed in claim 6, characterized in that: In the step 3), the exhaust gas is cooled by a heat exchanger and the incoming air is preheated at the same time. After the exhaust gas is cooled, it passes through a humus fixed bed to remove pollutant components in the gas, and is discharged into the air after being determined to meet the standards.

Citation Information

Patent Citations

  • Sintering swelled ultra-lightweight ceramsite produced by using silt and manufacturing method thereof

    CN104909816A

  • Preparation method of sheet materials with low pollution by using city sludge and calcium carbide slags

    CN105967752A

  • Method for preparing light calcium carbonate from carbide slag as raw material

    CN110078108A

  • Sludge mixed straw pyrolysis resource reduction method

    CN111253958A

  • Production method of biochar ceramsite particle filler

    CN115477527A