Photo-thermal glass and preparation method thereof

Through a specific ratio of raw materials and a multi-stage heating process, photothermal glass with high transmittance, excellent mechanical properties and thermal stability is prepared, which solves the problem of insufficient transmittance and mechanical properties in the production of photothermal glass and achieves Higher thermal stability and weathering resistance.

CN118851581APending Publication Date: 2024-10-29HENAN ANCAI PHOTOTHERMAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410756710.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Photothermal glass is difficult to achieve high transmittance and good mechanical properties during the production process, and it lacks thermal stability and weathering resistance, making it unable to meet the needs of solar water heaters, solar collectors and other fields.

Method used

It is composed of raw materials in a specific ratio, including silica, sodium oxide, calcium oxide, magnesium oxide, alumina, nano-zirconia, nano-zinc oxide and modified carbon nanotubes, and is prepared through a multi-stage heating process and annealing treatment. Produce photothermal glass with high transmittance, excellent mechanical properties and thermal stability.

Benefits of technology

It significantly improves the transmittance, mechanical strength and thermal stability of photothermal glass, extends its service life, avoids stress concentration caused by microbubbles and local overheating, and enhances the toughness and UV resistance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses photo-thermal glass and a preparation method thereof, and belongs to the technical field of glass, and the photo-thermal glass is prepared from the following raw materials in parts by weight: 60 to 70 parts of SiO2, 10 to 20 parts of Na2O, 5 to 10 parts of CaO, 2 to 4 parts of MgO, 4 to 8 parts of Al2O3, 0.5 to 1 part of ZrO2, 0.5 to 1 part of nano TiO2, 0.4 to 0.6 part of nano ZnO and 0.02 to 0.06 part of modified carbon nanotube. The photo-thermal glass prepared by the preparation method provided by the invention is high in light transmittance, good in mechanical property, good in thermal stability and long in service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of glass, and in particular relates to photothermal glass and a preparation method thereof. Background Art

[0002] As a special glass material, solar thermal glass has excellent photothermal performance and environmental protection characteristics, and has broad application prospects in the fields of solar energy utilization, building energy conservation, etc. In recent years, with the increasing global attention to renewable energy and environmental protection technology, the solar thermal glass industry has developed rapidly. In terms of technology research and development, the production process and technology of solar thermal glass have been continuously improved and innovated, improving the performance and quality of the product. At the same time, with the promotion and application of new energy technologies, the application of solar thermal glass in the fields of solar water heaters, solar collectors, etc. is becoming more and more extensive. In terms of market demand, with the improvement of people's awareness of environmental protection and energy conservation, and the support and promotion of government policies on renewable energy, the market demand for solar thermal glass continues to increase. Especially in the field of construction, solar thermal glass, as an effective energy-saving material, is favored by more and more architectural designers and developers.

[0003] Although the solar thermal glass industry has achieved remarkable development, there is still room for improvement in production processes and technologies, and challenges are still faced in achieving high efficiency, high quality, and high performance. One of the key technical indicators of solar thermal glass is that the transmittance of sunlight is ≥91%, especially for infrared light. The higher the transmittance, the more conducive it is to the reflection of solar thermal energy in plane mirrors or curved mirrors; but at present, due to the difficulty of clarifying solar thermal glass during the production process and the appearance of microbubbles in the glass, the transmittance and reflectivity of sunlight are directly affected, making the glass quality unable to meet the expected requirements. In the core components of solar thermal power stations such as heliostats, solar thermal glass needs to have good surface smoothness, bendability, and thermal strengthening properties, but there are still some deficiencies in this regard. In addition, solar thermal glass also needs to have strong weather resistance and weathering resistance to cope with harsh environmental conditions, such as ultraviolet radiation, high and low temperature cycles, etc., which is also the key point that current technology needs to break through.

[0004] Therefore, developing a photothermal glass with high transmittance, good mechanical properties and good thermal stability has become one of the problems that technical personnel in this field need to solve urgently. Summary of the invention

[0005] In view of this, the present invention discloses a photothermal glass and a preparation method thereof. The photothermal glass prepared by the preparation method provided by the present invention has high transmittance, good mechanical properties, good thermal stability and long service life.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] The invention provides a photothermal glass, which is composed of the following raw materials by weight: 60-70 parts of silicon dioxide SiO2, 10-20 parts of sodium oxide Na2O, 5-10 parts of calcium oxide CaO, 2-4 parts of magnesium oxide MgO, 4-8 parts of aluminum oxide Al2O3, 0.5-1 part of zirconium dioxide ZrO2, 0.5-1 part of nano titanium oxide TiO2, 0.4-0.6 part of nano zinc oxide ZnO, and 0.02-0.06 part of modified carbon nanotubes.

[0008] Preferably, the photothermal glass is composed of the following raw materials by weight: 65 parts of SiO2, 12 parts of Na2O, 7 parts of CaO, 3 parts of MgO, 6 parts of Al2O3, 0.6 parts of ZrO2, 0.6 parts of nano-TiO2, 0.5 parts of nano-ZnO, and 0.025 parts of modified carbon nanotubes.

[0009] Preferably, the preparation method of the modified carbon nanotubes is as follows: the carbon nanotubes are purified and pretreated, and the pretreated carbon nanotubes are added to a beaker containing an anhydrous ethanol solution of a silane coupling agent, and the beaker is placed on a constant temperature magnetic stirrer and heated and stirred at 70 to 80°C. After reacting for 2 to 3 hours, the mixture is filtered and washed, and then dried in a vacuum drying oven at 65 to 70°C to obtain the modified carbon nanotubes.

[0010] Preferably, the silane coupling agent is KH550, and the mass ratio of the silane coupling agent to anhydrous ethanol is (1-5):100.

[0011] Preferably, the mass ratio of the silane coupling agent to the carbon nanotubes is 1:(20-50).

[0012] The present invention also provides a method for preparing the above-mentioned photothermal glass, comprising the following steps:

[0013] S1. Prepare raw materials: weigh the raw materials in parts by weight, mix and grind to obtain a glass batch;

[0014] S2 melting: the glass batch obtained in step S1 is put into an electric melting furnace for melting, and the melt is melted, clarified, and homogenized to obtain a glass liquid;

[0015] S3 molding: the glass liquid obtained in step S2 is subjected to molding treatment to obtain a glass body;

[0016] S4. Finished product: After annealing and cooling, the glass blank obtained in step S3 is cut into finished glass of corresponding size, that is, photothermal glass is obtained.

[0017] Preferably, in step S2, the melting process of the electric melting furnace is set to four heating stages, and the temperature is increased from low to high according to the melting process, namely the first heating stage, the second heating stage, the third heating stage and the fourth heating stage; the maximum temperature of the first heating stage is 800-900°C, the maximum temperature of the second heating stage is 1400-1600°C, the maximum temperature of the third heating stage is 1400-1500°C, and the maximum temperature of the fourth heating stage is 1400-1500°C.

[0018] Preferably, in step S2, the insulation time of the first heating stage is 30 to 60 minutes, the insulation time of the second heating stage is 2 to 6 hours, the insulation time of the third heating stage is 5 to 8 hours, and the insulation time of the fourth heating stage is 5 to 8 hours.

[0019] Preferably, in step S4, the annealing process is: heating the glass body to 600-650°C at a rate of 1-2°C / min and keeping it warm for 30-60min, then heating it to 700-800°C at a rate of 2-3°C / min and keeping it warm for 120-240min, and finally cooling it to 30-40°C at a rate of 0.5-1°C / min.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) The annealing process provided by the present invention can slowly and evenly heat the formed glass body to the annealing temperature, ensuring uniform temperature distribution throughout the heating process, thereby effectively avoiding stress concentration caused by local overheating or overcooling, ensuring that internal stress can be effectively eliminated without damaging other properties of the glass.

[0022] (2) Under the premise of high transmittance of photothermal glass, the present invention adds a small amount of carbon nanotubes to its raw materials. The present invention uses a silane coupling agent to modify the carbon nanotubes. The silanol groups formed after hydrolysis of the silane coupling agent have high reactivity and can be connected with the functional groups on the surface of the carbon nanotubes through hydrogen bonds or covalent bonds, thereby anchoring the organic functional groups on the surface of the carbon nanotubes; on the other hand, the unreacted silanol groups can undergo condensation reactions with the hydroxyl groups on the surfaces of other glass raw materials under heating conditions to form stable silicon-oxygen bonds (Si-O-Si), or enhance the bonding force of the interface through hydrogen bond interactions; at the same time, the modified carbon nanotubes are easier to disperse evenly in the glass raw materials, which increases its compatibility with other glass raw materials and reduces interface defects. When the photothermal glass prepared by the present invention is subjected to external forces, the modified carbon nanotubes can effectively transfer the load as bridges, thereby significantly enhancing the mechanical properties of the overall material; at the same time, the modified carbon nanotubes dispersed in the glass matrix can serve as physical barriers. When the glass cracks due to external forces, the cracks may deflect or be terminated when encountering the nanotubes, thereby improving the toughness of the material. The modified carbon nanotubes in the present invention act on the photothermal glass through their own mechanical properties, dispersion morphology in the matrix, interface interaction with the matrix, and inhibition of crack expansion, thereby achieving a significant improvement in the mechanical strength and tensile strength of the photothermal glass.

[0023] (3) The present invention adds appropriate amounts of inorganic nanoparticles such as nano zinc oxide and nano titanium oxide, which can not only improve the mechanical strength and toughness of the photothermal glass, but also enhance its anti-ultraviolet and aging resistance, and improve the thermal stability and chemical resistance of the glass; at the same time, the present invention provides four heating zones in the process of preparing the photothermal glass, which correspond to the silicate heating formation stage, the glass liquid formation heating zone, the third glass liquid clarification heating zone and the glass liquid homogenization heating zone, which solves the problem that it is difficult to clarify and microbubbles are easy to appear in the glass during the current production process. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] The present invention provides a photothermal glass, which is composed of the following raw materials by weight: 60-70 parts of SiO2, 10-20 parts of Na2O, 5-10 parts of CaO, 2-4 parts of MgO, 4-8 parts of Al2O3, 0.5-1 part of ZrO2, 0.5-1 part of nano-TiO2, 0.4-0.6 part of nano-ZnO, and 0.02-0.06 part of modified carbon nanotubes.

[0026] The photothermal glass disclosed in the present invention is composed of the following raw materials according to the optimal weight proportions: 65 parts of SiO2, 12 parts of Na2O, 7 parts of CaO, 3 parts of MgO, 6 parts of Al2O3, 0.6 parts of ZrO2, 0.6 parts of nano-TiO2, 0.5 parts of nano-ZnO, and 0.025 parts of modified carbon nanotubes.

[0027] The preparation method of the modified carbon nanotubes of the present invention is as follows: the carbon nanotubes are purified and pretreated, and the pretreated carbon nanotubes are added into a beaker containing an anhydrous ethanol solution of a silane coupling agent KH550, and the beaker is placed on a constant temperature magnetic stirrer and heated and stirred at 70 to 80° C. After reacting for 2 to 3 hours, the mixture is filtered and washed, and then dried in a vacuum drying oven at 65 to 70° C. to obtain the modified carbon nanotubes.

[0028] The mass ratio of the silane coupling agent to anhydrous ethanol is (1-5):100, and the mass ratio of the silane coupling agent to the carbon nanotubes is 1:(20-50).

[0029] The present invention also provides a method for preparing the above-mentioned photothermal glass, comprising the following steps:

[0030] S1. Prepare raw materials: weigh raw materials according to weight ratio, mix and grind to obtain glass batch material.

[0031] S2. Melting: The glass batch material obtained in step S1 is put into an electric melting furnace for melting, and molten glass is obtained through melting, clarification and homogenization.

[0032] Among them, the melting processes of the electric melting furnace are the first heating stage, the second heating stage, the third heating stage and the fourth heating stage; the maximum temperature of the first heating stage is 800-900°C, the maximum temperature of the second heating stage is 1400-1600°C, the maximum temperature of the third heating stage is 1400-1500°C, and the maximum temperature of the fourth heating stage is 1400-1500°C; the insulation time of the first heating stage is 30-60min, the insulation time of the second heating stage is 2-6h, the insulation time of the third heating stage is 5-8h, and the insulation time of the fourth heating stage is 5-8h.

[0033] S3 molding: the glass liquid obtained in step S2 is subjected to molding treatment to obtain a glass body;

[0034] S4. Finished product: After annealing and cooling, the glass blank obtained in step S3 is cut into finished glass of corresponding size, that is, photothermal glass is obtained.

[0035] The annealing process is as follows: heating the glass blank to 600-650°C at a rate of 1-2°C / min and keeping it warm for 30-60min, then heating it to 700-800°C at a rate of 2-3°C / min and keeping it warm for 120-240min, and finally cooling it to 30-40°C at a rate of 0.5-1°C / min.

[0036] The technical solution of the present invention is further described below in conjunction with specific embodiments:

[0037] Example 1

[0038] The method for preparing the photothermal glass in this embodiment has the following specific steps:

[0039] S1. Prepare raw materials: prepare raw materials by weight: 65 parts of SiO2, 12 parts of Na2O, 7 parts of CaO, 3 parts of MgO, 6 parts of Al2O3, 0.6 parts of ZrO2, 0.6 parts of nano-TiO2, 0.5 parts of nano-ZnO, and 0.025 parts of modified carbon nanotubes, and mix and grind the raw materials to obtain a glass batch.

[0040] Among them, the preparation method of the modified carbon nanotubes in this embodiment is as follows: the carbon nanotubes are purified and pretreated, and the pretreated carbon nanotubes are added to a beaker containing an anhydrous ethanol solution of silane coupling agent KH550 (wherein, KH550: carbon nanotubes = 1:30, KH550: anhydrous ethanol = 3:100), and the beaker is placed on a constant temperature magnetic stirrer and heated and stirred at 75°C. After reacting for 2.5 hours, the modified carbon nanotubes are filtered and washed, and then dried in a vacuum drying oven at 70°C to obtain modified carbon nanotubes.

[0041] S2. Melting: Put the glass batch prepared in step S1 into an electric melting furnace for melting according to the melting process set in the electric melting furnace: the maximum temperature of the first heating stage is 900°C and the temperature is kept for 60 minutes, the maximum temperature of the second heating stage is 1500°C and the temperature is kept for 5 hours, the maximum temperature of the third heating stage is 1450°C and the temperature is kept for 6 hours, and the maximum temperature of the fourth heating stage is 1400°C and the temperature is kept for 7 hours; after melting, clarifying and homogenizing, glass liquid is obtained.

[0042] S3 molding: the glass liquid obtained in step S2 is subjected to molding treatment to obtain a glass body;

[0043] S4. Finished product: The glass blank obtained in step S3 is annealed by heating to 600°C at a rate of 1.5°C / min and keeping the temperature for 40 min, then heating to 750°C at a rate of 2.5°C / min and keeping the temperature for 200 min, and finally cooling to 35°C at a rate of 0.5°C / min. After annealing and cooling, the finished glass is cut into finished glass of corresponding size, that is, photothermal glass is obtained.

[0044] Example 2

[0045] The method for preparing the photothermal glass in this embodiment has the following specific steps:

[0046] S1. Prepare raw materials: prepare raw materials by weight: 60 parts of SiO2, 10 parts of Na2O, 8 parts of CaO, 2 parts of MgO, 8 parts of Al2O3, 1 part of ZrO2, 0.5 parts of nano-TiO2, 0.4 parts of nano-ZnO, and 0.02 parts of modified carbon nanotubes, and mix and grind the raw materials to obtain a glass batch.

[0047] Among them, the preparation method of the modified carbon nanotubes in this embodiment is as follows: the carbon nanotubes are purified and pretreated, and the pretreated carbon nanotubes are added to a beaker containing an anhydrous ethanol solution of silane coupling agent KH550 (wherein, KH550: carbon nanotubes = 1:20, KH550: anhydrous ethanol = 1:100), and the beaker is placed on a constant temperature magnetic stirrer and heated and stirred at 70°C. After reacting for 2 hours, the mixture is filtered and washed, and then dried in a vacuum drying oven at 65°C to obtain modified carbon nanotubes.

[0048] S2. Melting: Put the glass batch prepared in step S1 into an electric melting furnace for melting according to the melting process set in the electric melting furnace: the maximum temperature of the first heating stage is 800°C and the temperature is kept for 40 minutes; the maximum temperature of the second heating stage is 1600°C and the temperature is kept for 2 hours; the maximum temperature of the third heating stage is 1500°C and the temperature is kept for 5 hours; the maximum temperature of the fourth heating stage is 1450°C and the temperature is kept for 5 hours; after melting, clarifying and homogenizing, molten glass is obtained.

[0049] S3 molding: the glass liquid obtained in step S2 is subjected to molding treatment to obtain a glass body;

[0050] S4. Finished product: The glass blank obtained in step S3 is annealed by heating to 650°C at a rate of 1°C / min and keeping the temperature for 30 min, then heating to 700°C at a rate of 2°C / min and keeping the temperature for 120 min, and finally cooling to 30°C at a rate of 0.5°C / min. After annealing and cooling, the finished glass is cut into finished glass of corresponding size, that is, photothermal glass is obtained.

[0051] Example 3

[0052] The method for preparing the photothermal glass in this embodiment has the following specific steps:

[0053] S1. Prepare raw materials: prepare raw materials by weight: 70 parts of SiO2, 15 parts of Na2O, 5 parts of CaO, 4 parts of MgO, 6 parts of Al2O3, 0.5 parts of ZrO2, 1 part of nano-TiO2, 0.6 parts of nano-ZnO, and 0.04 parts of modified carbon nanotubes, and mix and grind the raw materials to obtain a glass batch.

[0054] Among them, the preparation method of the modified carbon nanotubes in this embodiment is as follows: the carbon nanotubes are purified and pretreated, and the pretreated carbon nanotubes are added to a beaker containing an anhydrous ethanol solution of silane coupling agent KH550 (wherein, KH550: carbon nanotubes = 1:50, KH550: anhydrous ethanol = 1:50), and the beaker is placed on a constant temperature magnetic stirrer and heated and stirred at 80°C. After reacting for 2 hours, the mixture is filtered and washed, and then dried in a vacuum drying oven at 65°C to obtain modified carbon nanotubes.

[0055] S2. Melting: Put the glass batch prepared in step S1 into an electric melting furnace for melting according to the melting process set in the electric melting furnace: the maximum temperature of the first heating stage is 850°C and the temperature is kept for 30 minutes, the maximum temperature of the second heating stage is 1400°C and the temperature is kept for 6 hours, the maximum temperature of the third heating stage is 1450°C and the temperature is kept for 7 hours, and the maximum temperature of the fourth heating stage is 1400°C and the temperature is kept for 8 hours; after melting, clarifying and homogenizing, glass liquid is obtained.

[0056] S3 molding: the glass liquid obtained in step S2 is subjected to molding treatment to obtain a glass body;

[0057] S4. Finished product: The glass blank obtained in step S3 is annealed by heating the glass blank to 650°C at a rate of 2°C / min and keeping the temperature for 60 min, then heating the glass blank to 800°C at a rate of 3°C / min and keeping the temperature for 240 min, and finally cooling the glass blank to 40°C at a rate of 1°C / min. After annealing and cooling, the glass blank is cut into finished glass of corresponding size, i.e., photothermal glass is obtained.

[0058] Example 4

[0059] The method for preparing the photothermal glass in this embodiment has the following specific steps:

[0060] S1. Prepare raw materials: prepare raw materials by weight: 70 parts of SiO2, 20 parts of Na2O, 6 parts of CaO, 3 parts of MgO, 8 parts of Al2O3, 0.5 parts of ZrO2, 1 part of nano-TiO2, 0.4 parts of nano-ZnO, and 0.06 parts of modified carbon nanotubes, and mix and grind the raw materials to obtain a glass batch.

[0061] Among them, the preparation method of the modified carbon nanotubes in this embodiment is as follows: the carbon nanotubes are purified and pretreated, and the pretreated carbon nanotubes are added to a beaker containing an anhydrous ethanol solution of silane coupling agent KH550 (wherein, KH550: carbon nanotubes = 1:20, KH550: anhydrous ethanol = 1:20), and the beaker is placed on a constant temperature magnetic stirrer and heated and stirred at 80°C. After reacting for 2 hours, the mixture is filtered and washed, and then dried in a vacuum drying oven at 65°C to obtain modified carbon nanotubes.

[0062] S2. Melting: Put the glass batch prepared in step S1 into an electric melting furnace for melting according to the melting process set in the electric melting furnace: the maximum temperature of the first heating stage is 900°C and the temperature is kept for 60 minutes, the maximum temperature of the second heating stage is 1600°C and the temperature is kept for 6 hours, the maximum temperature of the third heating stage is 1400°C and the temperature is kept for 8 hours, and the maximum temperature of the fourth heating stage is 1400°C and the temperature is kept for 8 hours; after melting, clarifying and homogenizing, glass liquid is obtained.

[0063] S3 molding: the glass liquid obtained in step S2 is subjected to molding treatment to obtain a glass body;

[0064] S4. Finished product: The glass blank obtained in step S3 is annealed by heating the glass blank to 650°C at a rate of 2°C / min and keeping the temperature for 60 min, then heating the glass blank to 800°C at a rate of 3°C / min and keeping the temperature for 240 min, and finally cooling the glass blank to 40°C at a rate of 1°C / min. After annealing and cooling, the glass blank is cut into finished glass of corresponding size, i.e., photothermal glass is obtained.

[0065] The photothermal glass prepared in the above examples 1-4 was tested. The transmittance was measured using a UV-2450 ultraviolet-visible spectrophotometer (550nm transmittance of photothermal glass). The thermal stability (°C) was measured using a vertical tubular electric furnace. In accordance with the standard SJ / T11037-1996, the bending test was measured using a QJ-211S universal testing machine. The samples used were all 1.0 mm thick. The test results are shown in Table 1.

[0066] Table 1

[0067]

[0068] The above is a detailed introduction to a photothermal glass and a preparation method thereof disclosed in the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method and core idea of ​​the present invention. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, several improvements and modifications can be made to the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A photothermal glass, characterized in that: The photothermal glass is composed of the following raw materials by weight: SiO2 60-70 parts, Na2O 10-20 parts, CaO 5-10 parts, MgO 2-4 parts, Al2O3 4-8 parts, ZrO2 0.5-1 part, nano-TiO2 0.5-1 part, nano-ZnO 0.4-0.6 part, modified carbon nanotubes 0.02-0.06 share.

2. The photothermal glass according to claim 1, characterized in that: The photothermal glass is composed of the following raw materials by weight: 65 parts of SiO2, 12 parts of Na2O, 7 parts of CaO, 3 parts of MgO, 6 parts of Al2O3 parts, 0.6 parts of ZrO2, 0.6 parts of nano-TiO2, 0.5 parts of nano-ZnO, and 0.025 parts of modified carbon nanotubes.

3. The photothermal glass according to claim 1, characterized in that: The preparation method of the modified carbon nanotubes is as follows: the carbon nanotubes are purified and pretreated, and the pretreated carbon nanotubes are added into a beaker containing an anhydrous ethanol solution of a silane coupling agent, and the beaker is placed on a constant temperature magnetic stirrer and heated and stirred at 70-80° C., and after reacting for 2-3 hours, the modified carbon nanotubes are filtered and washed, and then dried in a vacuum drying oven at 65-70° C. to obtain the modified carbon nanotubes.

4. The photothermal glass according to claim 3, characterized in that: The silane coupling agent is KH550, and the mass ratio of the silane coupling agent to anhydrous ethanol is (1-5):

100.

5. The photothermal glass according to claim 3, characterized in that: The mass ratio of the silane coupling agent to the carbon nanotubes is 1:(20-50).

6. The method for preparing photothermal glass according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1. Prepare raw materials: weigh the raw materials in parts by weight, mix and grind to obtain a glass batch; S2 melting: the glass batch obtained in step S1 is put into an electric melting furnace for melting, and the melt is melted, clarified, and homogenized to obtain a glass liquid; S3 molding: the glass liquid obtained in step S2 is subjected to molding treatment to obtain a glass body; S4. Finished product: After annealing and cooling, the glass blank obtained in step S3 is cut into finished glass of corresponding size, that is, photothermal glass is obtained.

7. The method for preparing photothermal glass according to claim 6, characterized in that: In step S2, the melting process of the electric melting furnace is set to four heating stages, and the temperature is increased from low to high according to the melting process, namely the first heating stage, the second heating stage, the third heating stage and the fourth heating stage; the maximum temperature of the first heating stage is 800-900°C, the maximum temperature of the second heating stage is 1400-1600°C, the maximum temperature of the third heating stage is 1400-1500°C, and the maximum temperature of the fourth heating stage is 1400-1500°C.

8. The method for preparing photothermal glass according to claim 7, characterized in that: In step S2, the insulation time of the first heating stage is 30 to 60 minutes, the insulation time of the second heating stage is 2 to 6 hours, the insulation time of the third heating stage is 5 to 8 hours, and the insulation time of the fourth heating stage is 5 to 8 hours.

9. The method for preparing photothermal glass according to claim 6, characterized in that: In step S4, the annealing process is: heating the glass body to 600-650°C at a rate of 1-2°C / min and keeping it warm for 30-60min, then heating it to 700-800°C at a rate of 2-3°C / min and keeping it warm for 120-240min, and finally cooling it to 30-40°C at a rate of 0.5-1°C / min.