Mesoporous silicon film loaded with ammonium phosphomolybdate as well as preparation method and application of mesoporous silicon film

By adsorbing and converting Cs+ into CsPbBr3 NCs loaded with ammonium phosphomolybdate mesoporous silicon films, the problem of in-situ separation of Cs+ enrichment and detection is solved, and efficient Cs+ fluorescence detection is achieved, which is suitable for the detection of complex matrix samples.

CN118851586APending Publication Date: 2024-10-29GUILIN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410817905.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The existing technology is difficult to achieve in-situ separation and detection after Cs+ enrichment, and porous materials are easily decomposed in water, affecting the growth of CsPbBr3 NCs.

Method used

Design a mesoporous silicon film loaded with ammonium phosphomolybdate, and load ammonium phosphomolybdate through the vertical mesoporous channel structure of the mesoporous silicon film to achieve selective adsorption and in-situ conversion of Cs+ into CsPbBr3 NCs, combined with a fluorescence detection strategy.

Benefits of technology

It achieves efficient enrichment and fluorescence detection of Cs+, reduces the detection limit of Cs+, is suitable for detecting Cs+ in complex matrix samples, and avoids the problem of decomposition of porous materials in water.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851586A_ABST
    Figure CN118851586A_ABST
Patent Text Reader

Abstract

The invention relates to an ammonium phosphomolybdate-loaded mesoporous silicon film as well as a preparation method and application thereof. The preparation method of the mesoporous silicon film loaded with the ammonium phosphomolybdate comprises the following steps: (1) synthesizing the mesoporous silicon film; and (2) loading ammonium phosphomolybdate to finally obtain the mesoporous silicon film loaded with ammonium phosphomolybdate. The mesoporous silicon film loaded with ammonium phosphomolybdate prepared by the invention has a vertical mesoporous channel structure, is loaded with ammonium phosphomolybdate, can selectively adsorb Cs < + >, and establishes a Cs < + > adsorption and detection integrated fluorescence sensing mode in combination with a fluorescence detection strategy of forming perovskite nanocrystals in situ. The invention also provides a fluorescence detection method for cesium ions in a water sample, which comprises the following steps: adsorbing enriched Cs < + > by the ammonium phosphomolybdate-loaded mesoporous silicon film, and converting the Cs < + > into fluorescent CsPbBr3NCs by using a PbBr2 solution, thereby establishing the fluorescence detection method for Cs < + >, and providing a new technology for detection of Cs < + > radionuclides in a complex matrix sample.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cesium ion enrichment and detection, and in particular to a mesoporous silicon film loaded with ammonium phosphomolybdate, and a preparation method and application thereof. Background Art

[0002] Heteropolyacids are a class of complex anions formed by inorganic polyacids (such as phosphate, silicate, tungstate, molybdate, etc.) connected by oxygen atoms, with unique structures and properties. Due to the good complexing ability, catalytic performance and adsorption performance of heteropolyacids, they are widely used in many fields. In the field of separation, heteropolyacid salts are widely used. By forming stable complexes with metal ions in the solution, they can achieve selective adsorption of specific ions, providing an effective method for applications such as ion exchange, ion removal, and metal extraction.

[0003] Ammonium phosphomolybdate (AMP) is a common heteropolyacid salt. Due to its stable Keggin-type heteropolyacid structure and more NH4 + , so that it can separate Cs by adsorption + When AMP is combined with Cs + When in contact, due to the active chemical properties of Cs, it can react with NH4 + In recent years, there have been a lot of studies on the adsorption of AMP on Cs + The research on the adsorption performance of AMP has achieved certain results. However, direct use of AMP powder to enrich Cs + After enrichment, it needs to be separated and recovered by centrifugation, which not only increases the sample processing time, but also easily leads to the loss of some AMP powder. In response to this, Xiaming Zheng's team coated ammonium phosphomolybdate in calcium alginate gel beads (ACCA) and used it to analyze Cs in soil. + Selective removal, adsorption capacity up to 39.75mg / g. ACCA on Cs in three different soils + The removal rates of AMP and Cs were 76%, 98% and 95% respectively. + The adsorption capacity of Cs + The adsorption efficiency can still reach more than 85%. By combining AMP with the gel, it can be quickly separated and recovered from the sample solution after the adsorption. However, the hydrogel has a high water content, and perovskite is easy to decompose in water. +After enrichment, it is impossible to in situ confine the growth of CsPbBr3 NCs in the hydrogel. Therefore, AMP is selected to load or composite with other porous materials to construct a new CsPbBr3 NCs by in situ spatial confinement growth strategy of perovskite nanocrystals. + Fluorescence detection methods are particularly important. Summary of the invention

[0004] Based on this, the object of the present invention is to provide a method for preparing a mesoporous silicon film loaded with ammonium phosphomolybdate, and the mesoporous silicon film loaded with ammonium phosphomolybdate in Cs + The present invention designs a mesoporous silicon film loaded with ammonium phosphomolybdate to detect Cs + The selective adsorption and fluorescence detection strategy of in-situ perovskite formation were established to detect Cs + The mesoporous silicon film loaded with ammonium phosphomolybdate of the present invention has a strong enrichment ability, which is conducive to reducing the detection limit of Cs+. + The ion exchange mechanism and enrichment performance of Cs + The ammonium phosphomolybdate-loaded mesoporous silica film was converted into CsPbBr3 NCs to establish Cs + Fluorescence detection method for Cs in complex matrix samples + Provides new technology for the detection of radionuclides.

[0005] The first aspect of the present invention is to provide a method for preparing a mesoporous silicon film loaded with ammonium phosphomolybdate, comprising the following steps:

[0006] (1) Synthesis of mesoporous silica films

[0007] Mix hexadecyltrimethylammonium chloride (CTAC), ethanol and n-decane in an ammonia solution, and stir at 50-70°C until transparent to form an oil-in-water emulsion; fix the polished quartz sheet in the groove of the template and immerse it in the oil-in-water emulsion; add a mixed solution of tetraethoxysilane and ethanol, stir and react at 50-70°C for 10-14h to obtain a glass slide; take out the glass slide, wash and dry it; calcine the dried glass slide at 530-570°C for 7-9h, remove the template, and obtain a mesoporous silicon film with quartz as the substrate;

[0008] (2) Loading of ammonium phosphomolybdate

[0009] Dissolve phosphomolybdic acid in water, immerse the mesoporous silicon film with quartz as the substrate therein, and stir evenly for 4-6 hours; add ammonium chloride and stir for 1-3 hours; take out the film product, wash and dry, and obtain the mesoporous silicon film with quartz as the substrate loaded with ammonium phosphomolybdate, that is, the mesoporous silicon film loaded with ammonium phosphomolybdate.

[0010] The preparation method of the mesoporous silicon film loaded with ammonium phosphomolybdate described in the present invention, in step (1), i.e., the synthesis method of the mesoporous silicon film, quartz is used as a substrate, and a mesoporous silicon film with a specific structure is grown on the quartz substrate by using an oil-induced co-assembly process. Wherein, the quartz sheet is fixed in the groove of the template to prevent the quartz sheet from moving due to stirring during the subsequent synthesis process; then immersed in the water-in-oil solution of hexadecyltrimethylammonium chloride-ethanol-n-decane-ammonia water, and a mixed solution of tetraethoxysilane and ammonia water is added; so that the quartz sheet is induced to form vertically arranged ordered micelles, and a mesoporous silicon film with vertical mesoporous channels is formed by calcination; that is, the mesoporous silicon film with quartz as the substrate obtained in step (1) has a vertical mesoporous channel structure. In step (1) of the present invention, i.e., the synthesis method of the mesoporous silicon film, the mesoporous silicon film grown on the quartz sheet has the properties of regular pore size, strong adjustability, large specific surface area and high porosity, and the mesoporous silicon film has good compatibility with the quartz substrate and is easy to grow on the quartz sheet. In addition, the mesoporous silicon film is easy to modify and modify, providing a good growth environment for the loading of ammonium phosphomolybdate (AMP), and can be easily compounded with ammonium phosphomolybdate (AMP). In step (2), i.e., the loading method of ammonium phosphomolybdate, ammonium phosphomolybdate is generated in the vertical mesoporous channels of the mesoporous silicon film with quartz as the substrate, so that the ammonium phosphomolybdate is loaded on the mesoporous silicon film. Among them, the mesoporous silicon film with quartz as the substrate is first placed in the phosphomolybdic acid solution, so that the vertical mesoporous channels are filled with the phosphomolybdic acid solution; after adding ammonium chloride and stirring, ammonium phosphomolybdate is generated in the vertical mesoporous channels, and a mesoporous silicon film loaded with ammonium phosphomolybdate on the quartz substrate is obtained, i.e., the mesoporous silicon film loaded with ammonium phosphomolybdate. Preferably, in step (1), the size of the quartz sheet is 1.3 cm×1.3 cm.

[0011] Furthermore, in step (2), the mass ratio of phosphomolybdic acid to ammonium chloride is 1:1.

[0012] Furthermore, the amount of phosphomolybdic acid and ammonium chloride used is 30-70 mg. Preferably, the amount of phosphomolybdic acid and ammonium chloride used is 50 mg and 50 mg (1:1). When the amount of phosphomolybdic acid and ammonium chloride used is 50 mg and 50 mg (1:1), the prepared mesoporous silicon film loaded with ammonium phosphomolybdate has a good effect on Cs + The enrichment effect of ammonium phosphomolybdate was the best; when the amount exceeded 50 mg, the prepared mesoporous silicon film loaded with ammonium phosphomolybdate had a good enrichment effect on Cs + The adsorption amount did not change much.

[0013] The second aspect of the present invention is to provide a mesoporous silicon film loaded with ammonium phosphomolybdate prepared by any of the above methods for preparing a mesoporous silicon film loaded with ammonium phosphomolybdate.

[0014] The mesoporous silicon film loaded with ammonium phosphomolybdate prepared by the present invention has a vertical mesoporous channel structure and is loaded with ammonium phosphomolybdate, which is Cs + The in-situ adsorption of AMP and in-situ growth of CsPbBr3 NCs provide feasibility. The mesoporous silicon film loaded with ammonium phosphomolybdate prepared by the present invention can in-situ adsorb and enrich Cs+; the ammonium phosphomolybdate (AMP) on the mesoporous silicon film loaded with ammonium phosphomolybdate has a unique Keggin structure, which enables AMP to effectively bind to cesium ions (Cs + ) undergoes ion exchange. In the Keggin structure of AMP, the position of [P(MO 12 O 40 )] 3- NH4 in the anion gap of a hollow sphere + Can be used with Cs + exchange. Since [P(MO 12 O 40 )] 3- Anion gap size limitation and O and Cs + The strong coordination ability between Cs + In addition, the mesoporous silicon film loaded with ammonium phosphomolybdate is enriched with Cs + After that, Cs + In situ growth of fluorescent CsPbBr3 NCs provides the possibility for fluorescence detection. The mesoporous silicon film loaded with ammonium phosphomolybdate prepared by the present invention uses a quartz sheet as a substrate. Quartz has good light transmittance and almost no light absorption in the visible light range, which is conducive to the use of the prepared mesoporous silicon film loaded with ammonium phosphomolybdate for Cs + Fluorescence detection can prevent the substrate from absorbing part of the fluorescence, which will lead to a decrease in the sensitivity of cesium ion detection.

[0015] The third aspect of the present invention is to provide a mesoporous silicon film loaded with ammonium phosphomolybdate as described above on Cs + The mesoporous silicon film loaded with ammonium phosphomolybdate prepared by the present invention is used for enrichment of Cs + Selective adsorption, suitable for enriching radioactive nuclide Cs from complex matrix samples + .

[0016] The fourth aspect of the present invention is to provide a mesoporous silicon film loaded with ammonium phosphomolybdate as described above on Cs + Application in fluorescence detection. Adsorption of Cs by mesoporous silica film loaded with ammonium phosphomolybdate + , and converted into substances with fluorescent properties for fluorescence detection.

[0017] The fifth aspect of the present invention is to provide a method for detecting cesium ions (Cs +) Fluorescence detection method, comprising the following steps:

[0018] S1, Cs + Adsorption

[0019] Take any of the above-mentioned mesoporous silicon films loaded with ammonium phosphomolybdate, add them to the water sample, stir and adsorb the cesium ions (Cs + ); taking out the adsorbed film, rinsing and drying;

[0020] S2. In situ growth of CsPbBr3 NCs

[0021] PbBr2 solution was added dropwise onto the dried film of S1 and dried;

[0022] S3. Fluorescence detection

[0023] The S2 film was dried and subjected to fluorescence detection.

[0024] The present invention utilizes the mesoporous silicon film loaded with ammonium phosphomolybdate to treat Cs + The selective adsorption of Cs + The invention relates to a fluorescence sensing mode integrating adsorption and detection. + ) fluorescence detection method, by adsorbing the enriched Cs + The fluorescent CsPbBr3 NCs were converted into CsPbBr3 NCs by using PbBr2 solution, and the fluorescence intensity of CsPbBr3 NCs was similar to that of Cs in water samples. + The concentration of Cs + Fluorescence detection method for Cs in complex matrix samples + Provides new technology for the detection of radionuclides.

[0025] Furthermore, in S1, the adsorption time is 15-120 min. Preferably, the adsorption time is 15 min. The mesoporous silicon film loaded with ammonium phosphomolybdate of the present invention has an adsorption capacity of Cs + The adsorption rate is fast, and the equilibrium can be reached after 15 min of adsorption. Therefore, in order to shorten the experimental and analysis time, Cs + The adsorption time was controlled at 15min.

[0026] Further, in S1, the pH of the water sample is adjusted to 3-6. That is, cesium ion (Cs + ) adsorption; the present invention found that the loaded ammonium phosphomolybdate mesoporous silicon film (AMP-SiO2 film) at pH 3-6 conditions, the Cs + It has excellent adsorption effect and has a good adsorption effect on Cs +The adsorption change of CsPbBr3 NCs was small, and the PL intensity of the formed CsPbBr3 NCs was also close. When pH>6, the mesoporous silicon film loaded with ammonium phosphomolybdate (AMP-SiO2 film) had a strong effect on Cs + The adsorption capacity of CsPbBr3 NCs was significantly weakened, and the PL intensity was greatly weakened after derivatization. When the pH was alkaline, the NH4 + Will react with OH in water - Reaction, OH - With Cs + Competitive adsorption occurs, thus weakening the adsorption capacity, resulting in a significant decrease in fluorescence intensity during fluorescence detection. When pH < 3, under strong acidic conditions (pH < 3) for a long time, the ammonium phosphomolybdate on the film will decompose to produce ammonium molybdate, phosphoric acid and nitrogen dioxide, and the number of ammonium phosphomolybdate molecules will decrease, resulting in the Cs + The number of binding sites is reduced, resulting in a decrease in the amount of adsorption. Secondly, the film is easy to fall off from the quartz sheet under strong acid conditions for a long time, and the material is damaged. Both of these situations lead to the enrichment of Cs in the material. + Therefore, the present invention performs adsorption in the range of pH 3-6, so that the adsorption capacity of the mesoporous silicon film loaded with ammonium phosphomolybdate remains stable, and the fluorescence intensity finally generated is strong. Preferably, the adsorption is performed under the condition of pH 3. At pH 3, the mesoporous silicon film loaded with ammonium phosphomolybdate has a strong adsorption capacity for Cs + The adsorption effect is the best, the adsorption amount reaches the maximum, and the subsequent fluorescence intensity is the highest.

[0027] Furthermore, in S1, the volume of the water sample is 10-150 ml. When the volume of the water sample (adsorption volume) is within the range of 10-150 mL, the mesoporous silicon film loaded with ammonium phosphomolybdate has an adsorption capacity of Cs + The adsorption effect is good, and the adsorption amount and the fluorescence intensity generated by CsPbBr3 NCs are stable.

[0028] Further, in S2, the concentration of the PbBr2 solution is 0.01-0.05 mol / L. Preferably, the concentration of the PbBr2 solution is 0.03 mol / L. A lower PbBr2 concentration cannot completely convert Cs+ into CsPbBr3 NCs, while a higher concentration of PbBr2 easily leads to the generation of some non-fluorescent CsPb2Br5 NCs during the growth of CsPbBr3 NCs, which reduces the number of CsPbBr3 NCs and leads to a decrease in fluorescence intensity.

[0029] Further, in S3, the specific method of fluorescence detection includes the following steps: preparing Cs + Concentration 0.0005-30μgmL -1The multiple cesium carbonate standard solutions were used as standard water samples to perform steps S1 and S2 respectively, and the fluorescence intensity of CsPbBr3 NCs was measured. + The concentration of CsPbBr3NCs in the water sample to be tested is plotted as a standard working curve; the water sample to be tested is taken to perform steps S1 and S2, and the fluorescence intensity of CsPbBr3NCs measured is substituted into the above standard working curve to obtain the concentration of Cs + concentration.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] The present invention designs a mesoporous silicon film loaded with ammonium phosphomolybdate to + The selective adsorption of Cs + The mesoporous silicon film loaded with ammonium phosphomolybdate of the present invention has a stronger enrichment ability and is beneficial to reduce Cs + The present invention is to enrich Cs in a mesoporous silicon film loaded with ammonium phosphomolybdate. + Conversion into CsPbBr3 NCs to build Cs + Fluorescence detection method for Cs in complex matrix samples + Provides new technology for the detection of radionuclides.

[0032] For better understanding and implementation, the present invention is described in detail below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 Adsorption of Cs on AMP-SiO2 films + Schematic diagram of the process and in-situ growth of CsPbBr3 NCs;

[0034] Figure 2 SEM image of the peeled SiO2 film (a), TEM top view of the enlarged SiO2 film (b), TEM image of CsPbBr3NCs-AMP-SiO2 (c) and lattice fringes (d);

[0035] Figure 3 XRD spectra of SiO2 film, AMP-SiO2 film and CsPbBr3 NCs-AMP-SiO2 film;

[0036] Figure 4 Wide scan XPS spectra of SiO2 film, AMP-SiO2 film, AMP-SiO2-Cs film, CsPbBr3-AMP-SiO2 film (a), Cs3d (b), Pb 4f (c), and Br 3d (d);

[0037] Figure 5 PL spectra of CsPbBr3NCs crystallized in mesoporous silicon films loaded with different masses of phosphomolybdic acid and ammonium chloride (1:1) (a), PL intensity and Cs + Variation of adsorption amount with the amount of phosphomolybdic acid and ammonium chloride used (b);

[0038] Figure 6 Cs + Variation of adsorption amount on AMP-SiO2 film with adsorption time;

[0039] Figure 7 PL spectra of CsPbBr3 NCs crystallized on AMP-SiO2 under different pH solutions (a), PL intensity and Cs + Variation of adsorption amount with pH (b);

[0040] Figure 8 (a) PL spectra of CsPbBr3 NCs crystallized on AMP-SiO2 at adsorption volumes of 10-250 mL. The PL intensity increases with the adsorption of Cs + Change of adsorption amount and adsorption volume (b);

[0041] Fig. 9 (a) PL spectra of CsPbBr3 NCs in PbBr2 solutions with different concentrations, PL intensity and Cs + Variation of adsorption amount with the concentration of PbBr2 solution (b);

[0042] Fig.10 Adsorption of Cs on AMP-SiO2 films + Langmuir (a) and Freundlich (b) isotherm models;

[0043] Fig.11 Adsorption of Cs on AMP-SiO2 films + Pseudo-first-order adsorption kinetics (a) and pseudo-second-order adsorption kinetics (b);

[0044] Fig.12 For CsPbBr3 NCs at different concentrations of Cs + PL spectra in the presence of (a) and the corresponding enhanced PL intensity (b), PL peak wavelength shift (c);

[0045] Fig.13 For CsPbBr3 NCs in Cs + The relative fluorescence intensity in the presence of Cs + Concentration 1 μg mL -1 , other ions are 10 μg mL -1 or 15 μg mL -1 . DETAILED DESCRIPTION

[0046] The present invention is described in detail below by specific embodiments and accompanying drawings. Unless otherwise specified, the technical means used in the present invention are methods known to those skilled in the art. In addition, the embodiments should be understood as illustrative rather than limiting the scope of the present invention, and the essence and scope of the present invention are limited only by the claims. For those skilled in the art, without departing from the essence and scope of the present invention, various changes or modifications of the material composition and dosage in these embodiments also belong to the protection scope of the present invention.

[0047] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0048] The first aspect of the embodiment of the present invention is to provide a method for preparing a mesoporous silicon film (AMP-SiO2 film) loaded with ammonium phosphomolybdate, comprising the following steps:

[0049] (1) Synthesis of mesoporous silica films

[0050] Mix hexadecyltrimethylammonium chloride (CTAC), ethanol and n-decane in an ammonia solution, and stir at 50-70°C until transparent to form an oil-in-water emulsion; fix the polished quartz sheet in the groove of the template and immerse it in the oil-in-water emulsion; add a mixed solution of tetraethoxysilane and ethanol, stir and react at 50-70°C for 10-14h to obtain a glass slide; take out the glass slide, wash and dry it; calcine the dried glass slide at 530-570°C for 7-9h, remove the template, and obtain a mesoporous silicon film with quartz as the substrate;

[0051] (2) Loading of ammonium phosphomolybdate

[0052] Dissolve phosphomolybdic acid in water, immerse the mesoporous silicon film with quartz as the substrate therein, and stir evenly for 4-6 hours; add ammonium chloride and stir for 1-3 hours; take out the film product, wash and dry, and obtain the mesoporous silicon film with quartz as the substrate loaded with ammonium phosphomolybdate, that is, the mesoporous silicon film loaded with ammonium phosphomolybdate.

[0053] In the embodiment of the present invention, the size of the quartz sheet is 1.3cm×1.3cm; the template is a polytetrafluoroethylene template, and the polytetrafluoroethylene template is provided with a groove matching the size of the quartz sheet. The template is provided with a groove matching the size of the quartz sheet, so as to fix the quartz sheet in the groove of the template and prevent the quartz sheet from moving due to stirring during the subsequent synthesis process. It should be noted in the present application that the groove of the template is also commonly referred to as a hole in the art, and in the present invention it can also refer to: a polytetrafluoroethylene template after opening a hole (square channel: 1.3cm×1.3cm, thickness 0.2cm).

[0054] The second aspect of the embodiment of the present invention is to provide a mesoporous silicon film loaded with ammonium phosphomolybdate prepared by the above preparation method.

[0055] The third aspect of the embodiment of the present invention is to provide a mesoporous silicon film loaded with ammonium phosphomolybdate on Cs + Application in adsorption.

[0056] A fourth aspect of the embodiment of the present invention is to provide a mesoporous silicon film loaded with ammonium phosphomolybdate on Cs + Applications in fluorescence detection.

[0057] A fifth aspect of the present invention is to provide a method for detecting cesium ions (Cs + ) Fluorescence detection method, comprising the following steps:

[0058] S1, Cs + Adsorption

[0059] Take any of the above-mentioned mesoporous silicon films loaded with ammonium phosphomolybdate (AMP-SiO2 film), add it to the water sample, stir and adsorb cesium ions (Cs + ); taking out the adsorbed film, rinsing and drying;

[0060] S2. In situ growth of CsPbBr3 NCs

[0061] PbBr2 solution was added dropwise onto the dried film of S1 and dried;

[0062] S3. Fluorescence detection

[0063] The S2 film was dried and subjected to fluorescence detection.

[0064] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.

[0065] Example 1

[0066] 1. Experimental part

[0067] 1.1 Experimental Reagents

[0068] Table 1 Reagents used in this experiment

[0069]

[0070] 1.2 Synthesis method of mesoporous silica film

[0071] CTAC (0.193 g), ethanol (6.0 g) and n-decane (600 μL) were mixed in an ammonia solution (0.4 mol / L, 80 g) and stirred at 60 °C until transparent to form an oil-in-water emulsion; then a polished quartz sheet (1.3 cm × 1.3 cm) was fixed on a polytetrafluoroethylene template with a hole (square channel: 1.3 cm × 1.3 cm, thickness 0.2 cm), and then immersed in the above oil-in-water emulsion, and then a mixed solution of TEOS (400 μL) and ethanol (1.2 mL) was added, and mechanically stirred at 60 °C for 12 h to obtain a glass slide. After stirring, the glass slide was taken out, rinsed three times with secondary water, and dried at 60 °C. The dried glass slide was taken out and calcined in a 550 °C tube furnace for 8 h to remove the template, and cooled to obtain a mesoporous silicon film based on quartz, referred to as SiO2 film.

[0072] 1.3 Loading of ammonium phosphomolybdate

[0073] Weigh 50 mg of phosphomolybdic acid and dissolve it in 10 mL of secondary water, immerse the mesoporous silicon film (SiO2 film) based on quartz, stir at a constant speed for 5 hours, then add 50 mg of ammonium chloride and stir for 2 hours. After stirring, rinse the quartz sheet with secondary water and dry it at 60°C for 2 hours to obtain a mesoporous silicon film loaded with ammonium phosphomolybdate based on quartz, that is, the mesoporous silicon film loaded with ammonium phosphomolybdate, referred to as AMP-SiO2 film.

[0074] 1.4Cs + Adsorption and in situ growth of CsPbBr3 NCs

[0075] The quartz-based mesoporous silicon film loaded with ammonium phosphomolybdate (AMP-SiO2 film) was placed in a centrifuge tube containing 10 mL of H2O and 100 μL of 3.93 mg mL -1 Cs2CO3(0.3mg mL -1 Cs +). After 15 minutes of stirring and adsorption, the film was taken out, rinsed with clean water three times, and then vacuum dried at 160℃ for 10 minutes to obtain AMP-SiO2-Cs film; 100μL of the remaining adsorbed liquid was used for graphite furnace atomic absorption detection. The dried AMP-SiO2-Cs film was taken out and 10μL of 3mmol / L PbBr2 solution (N-methylformamide as solvent) was added to the film. After being placed in a natural environment for 5 minutes, it was vacuum dried at 150℃ for 10 minutes to obtain CsPbBr3 NCs-AMP-SiO2 film. The film was cooled to room temperature in a vacuum environment and then taken out for fluorescence measurement.

[0076] 1.5 Actual sample analysis

[0077] Weigh 1 mg mL -1 The cesium carbonate standard stock solutions were prepared into 30 μg mL -1 , 20 μg mL -1 , 15 μg mL -1 , 10 μg mL -1 , 5 μg mL -1 , 1 μg mL -1 , 0.5 μg mL -1 , 0.1 μg mL -1 , 0.05 μg mL -1 , 0.001μg mL -1 Then add AMP-SiO2 film and perform Cs + The adsorption and growth of CsPbBr3 NCs were investigated based on the fluorescence intensity of CsPbBr3 NCs. + A standard working curve was drawn based on the concentrations of .

[0078] The actual samples were taken from seawater samples in Beihai and Fangchenggang, Guangxi. First, 20 mL of water sample was filtered with a 0.22 μm filter. AMP-SiO2 film was added to the filtrate, magnetically stirred and adsorbed for 10 min, and rinsed three times. Cs + The standard solution was added to the water sample for recovery experiment.

[0079] 1.6 Characterization Instrument Use

[0080] X-ray photoelectron spectroscopy (XPS) was collected by Thermo Scientific K-Alpha, USA. Infrared spectra (FTIR) were collected using a Nicolet IS10FTIR spectrometer (Thermo Fisher scientific Co, USA). The morphology of SiO2 film, AMP-SiO2 film, and CsPbBr3 NCs-AMP-SiO2 film was observed using a JEM 2000F transmission electron microscope (TEM) (JEOL, Japan). The crystal form of CsPbBr3 NCs-AMP-SiO2 was characterized using an X'pert Pro (PANalytical Ltd, Netherlands) X-ray powder diffractometer (XRD). Fluorescence (PL) spectra were recorded on a Hitachi F-7000 fluorescence spectrophotometer with an excitation wavelength of 365 nm. The excitation and emission slit widths were 1.0 nm and 2.5 nm, respectively. The detection method was verified using a Pulse TAS990 graphite furnace atomic absorption spectrometer (drying temperature: 100°C, ashing temperature: 400°C, atomization temperature: 1900°C, residue removal temperature: 2200°C, injection volume: 10 μL).

[0081] 2. Results and Discussion

[0082] 2.1Cs + Enrichment and in situ growth mechanism of CsPbBr3 NCs

[0083] See also Figure 1 In this method, AMP-SiO2 thin film is used to treat Cs + Ammonium phosphomolybdate (AMP) has a unique Keggin structure, which enables AMP to effectively bind to cesium ions (Cs + ) undergoes ion exchange. In the Keggin structure of AMP, the position of [P(MO 12 O 40 )] 3- NH4 in the anion gap of a hollow sphere + Can be used with Cs + exchange. Since [P(MO 12 O 40 )] 3- Anion gap size limitation and O and Cs + The strong coordination ability between Cs + Selective exchange. When enriched with Cs + After that, the load Cs + The dried AMP-SiO2 film was completely impregnated with an appropriate amount of PbBr2 solution, and then dried naturally and fully dried to crystallize into CsPbBr3 NCs. The fluorescence intensity of CsPbBr3 NCs is similar to that of Cs in the original solution.+ The concentration of Cs + Fluorescence detection method; at the same time, because AMP-SiO2 film is used as the adsorption substrate, the enrichment multiple of AMP-SiO2 film is high, which is beneficial to reduce Cs + Detection limit.

[0084] 2.2 Material characterization

[0085] AMP-SiO2 thin film is based on quartz wafers. The oil-induced co-assembly process is used to grow mesoporous silicon thin films on quartz substrates. Please refer to Figure 2 (a) is a SEM image of a peeled SiO2 film (the quartz substrate has poor conductivity, so the image is not clear if it is taken with the quartz substrate attached, so the grown mesoporous silicon film is peeled off). The grown mesoporous silicon film has a uniform thickness of about 55nm and has a vertical pore structure; please refer to Figure 2 (b) is a magnified TEM top view of the SiO2 film. It can be seen that the mesopores on the film are densely distributed with a pore size of about 4nm, providing a good growth environment for the loading of AMP and perovskite nanocrystals CsPbBr3 NCs. As shown in the TEM image, AMP and CsPbBr3 NCs have been successfully crystallized in the mesopores, and the lattice fringe spacing corresponding to the CsPbBr3 (220) crystal plane is clearly observed to be 0.20nm, and the lattice fringe spacing corresponding to the AMP (322) crystal plane is 0.25nm, see Figure 2 (c) and 2(d).

[0086] X-ray diffractometer (XRD) was used to characterize SiO2 film, AMP-SiO2 film and CsPbBr3-AMP-SiO2 film after in-situ growth of perovskite. Figure 3 , which are SiO2 thin films, AMP-SiO2 thin films, CsPbBr 3- XRD spectrum of AMP-SiO2 film. The XRD spectrum of SiO2 film only shows a broad peak in the 2θ angle range of 15-30°, indicating the amorphous state of SiO2 film. The strong diffraction peaks of AMP-SiO2 film at 2θ=10.7°, 16.2°, 21.5°, 26.3°, 30.5°, and 36.3° belong to the (110), (211), (220), (222), (400), and (322) crystal planes of Keggin-type compound structure. After comparison with the standard card, these crystal planes belong to ammonium phosphomolybdate, proving that AMP has been successfully loaded onto the mesoporous silicon film. Enriched Cs + After that, the XRD pattern of the in-situ converted CsPbBr3 NC (i.e., CsPbBr 3-The XRD spectrum of AMP-SiO2 film shows that the previously unknown (100), (200), and (210) planes appear at 14.9°, 29.5°, and 33.7°. These planes belong to CsPbBr3 NCs, proving that AMP-SiO2 film adsorbs Cs + At the same time, we found that after the in situ conversion of CsPbBr3 NCs, the characteristic peak of ammonium phosphomolybdate (AMP) did not disappear. We speculate that ammonium phosphomolybdate has a certain effect on the CsPbBr3 NCs. + During adsorption, the phosphomolybdic acid on the ammonium phosphomolybdate does not participate in the adsorption process, but only NH4 + With Cs + exchange, and only part of NH4 + Participate in the exchange, so ammonium phosphomolybdate does not completely disappear, and the corresponding characteristic peak of ammonium phosphomolybdate still exists. At the same time, when the concentration of lead bromide added is too much, the characteristic peak of CsPb2Br5 appears at 11.12°, so the concentration of PbBr2 needs to be optimized in the later stage to obtain a stable ABX3 perovskite.

[0087] See also Figure 4 We used AMP-SiO2 film, AMP-SiO2-Cs film and CsPbBr 3- XPS data of AMP-SiO2 film to further explore the relationship between ammonium phosphomolybdate and Cs + The ion exchange mechanism of Cs + The valence state of CsPbBr3 is changed. Figure 4 (a) It can be seen that after loading phosphomolybdic acid, N1s, P 2p, and Mo 3d signals appeared on the AMP-SiO2 film, which once again proved that ammonium phosphomolybdate has been successfully loaded on the mesoporous silicon film (SiO2 film). + After AMP-SiO2-Cs film was treated with ammonium phosphomolybdate, the N1s content of AMP-SiO2-Cs film decreased, while the Cs 3d content increased, and the P 2p and Mo 3d contents did not change much (see Table 2). This phenomenon verified our previous speculation that ammonium phosphomolybdate has a significant effect on Cs + During the adsorption process, only NH4 + With Cs + exchange. And from the N1s content of AMP-SiO2-Cs film, it can be known that NH4 + Although it is exchanged, some of it still remains, and its exchange reaction is as follows:

[0088]

[0089] And through Figure 4(b) It can be seen that after in situ conversion of CsPbBr3 NCs, Cs 3d 3 / 2 The binding energy of Cs 3d increases from 723.18 eV to 724.38 eV. 5 / 2 The energy level of Cs increases from 737.08eV to 738.38eV, indicating that + After conversion to CsPbBr3NCs, the binding energy becomes larger and the electron cloud density increases, which is caused by the combination of Cs with Br and Pb, proving the success of in-situ conversion of CsPbBr3NCs. Figure 4 (c) and Figure 4 (d) It can be seen that the morphology of Pb and Br is also the corresponding morphology in CsPbBr3 NCs, which also proves the successful crystallization of CsPbBr3 NCs.

[0090] Table 2 Atomic contents of AMP-SiO2 and AMP-SiO2-Cs obtained by XPS analysis

[0091]

[0092] 2.3Cs + Optimization of adsorption and derivatization conditions of CsPbBr3 NCs

[0093] The loading amount of ammonium phosphomolybdate, pH, adsorption volume and the amount of PbBr2 used may affect the adsorption of AMP-SiO2 films on Cs + It affects the enrichment and growth of CsPbBr3 NCs and needs to be optimized.

[0094] (1) Optimization of ammonium phosphomolybdate loading

[0095] Since the actual mass of AMP loaded on the AMP-SiO2 film is difficult to measure accurately, the amount of phosphomolybdic acid and ammonium chloride used when loaded with ammonium phosphomolybdate is optimized (the amount used refers to the amount used relative to each piece of AMP-SiO2 film). In the experiment, the mass ratio of phosphomolybdic acid and ammonium chloride was kept at 1:1 to ensure that the phosphomolybdic acid was excessive. + The optimal amount of phosphomolybdic acid and ammonium chloride was determined by the adsorption amount and the PL intensity of CsPbBr3 NCs. Figure 5 (b) It can be seen that when the amount of phosphomolybdic acid and ammonium chloride used is 50 mg and 50 mg (1:1), the film loaded with ammonium phosphomolybdate has a significant effect on the Cs + The enrichment effect is the best. When the usage exceeds 50 mg, the adsorption amount does not change much. It can be determined that the best usage for loading ammonium phosphomolybdic acid is to use 50 mg phosphomolybdic acid and 50 mg ammonium chloride. At the same time, according to the PL fluorescence intensity diagram of in-situ grown perovskite nanocrystals CsPbBr3 NCs ( Figure 5(a) As can be seen from the figure, when the amount of phosphomolybdic acid and ammonium chloride increases, the fluorescence intensity also increases. It can be judged that the fluorescence intensity of perovskite nanocrystals is related to the adsorption of Cs + Quantity is positively correlated.

[0096] (2) For Cs + The adsorption amount and adsorption time were optimized.

[0097] See also Figure 6 It can be seen that AMP-SiO2 film has a great influence on Cs + The adsorption of Cs + The adsorption amount of AMP-SiO2 film was 323 μg / piece. When the adsorption time was extended to 120 min, the adsorption amount increased to 345 μg / piece, which was only 7% higher. Therefore, in the subsequent experiments, in order to shorten the experimental and analysis time, Cs + The adsorption time was controlled at 15min.

[0098] (3) For Cs + Optimization of pH for adsorption

[0099] Since the pH of the solution often affects the adsorption process, this example investigates the adsorption of Cs by AMP-SiO2 film in solutions with pH values ​​ranging from 1 to 10. + The adsorption of Figure 7 (a) and Figure 7 As shown in (b), at pH 3, Cs + The adsorption effect is the best, the adsorption amount reaches the maximum, and the PL intensity is the highest. In the pH range of 3-6, AMP-SiO2 film has a good adsorption effect on Cs + The adsorption of CsPbBr3 NCs changes little, so the PL intensity is close after forming CsPbBr3 NCs. + The adsorption capacity of CsPbBr3 NCs was significantly weakened, and the PL intensity was greatly weakened after derivatization. Under strong acidic conditions (pH < 3) for a long time, ammonium phosphomolybdate will decompose to produce ammonium molybdate, phosphoric acid and nitrogen dioxide, and the number of ammonium phosphomolybdate molecules will decrease, resulting in the Cs + The number of binding sites is reduced, resulting in a decrease in the amount of adsorption. Secondly, the film material is easy to fall off from the quartz sheet under strong acid conditions for a long time, and the material is damaged. Both of these situations lead to the enrichment of Cs in the material. + Under alkaline conditions, the sharp decrease in fluorescence intensity is due to the NH4 + Will react with OH in water - Reaction, OH - With Cs +Competitive adsorption occurs, thus weakening the adsorption capacity. Given that the adsorption capacity of the material remains stable within the pH range of 3-6, and the resulting fluorescence intensity is relatively strong, subsequent experiments were conducted under the condition of pH 3.

[0100] (4) For Cs + Optimize the adsorption volume during adsorption

[0101] In order to test the effect of AMP-SiO2 film on Cs + The enrichment capacity of AMP-SiO2 thin film materials for Cs + See Figure 8 (a) and (b), the adsorption volume is 10-250 mL (both containing 0.300 mg Cs + ), when the adsorption volume ranges from 10 to 150 mL, Cs + There was no significant decrease in the adsorption amount and fluorescence intensity of CsPbBr3 NCs. When the volume increased from 150mL to 250mL, the PL intensity decreased significantly, and the PL intensity decreased by about 40%, indicating that as the adsorption volume was too large, the AMP-SiO2 film was more sensitive to CsPbBr3 NCs. + The adsorption capacity is weakened. By calculation, the corresponding enrichment factors of 10mL to 250mL are 4390, 10909, 10909, 42613, 62500, and 61289, respectively. Therefore, the optimal adsorption volume is 150mL.

[0102] (5) Optimize the usage of PbBr2

[0103] During the growth of CsPbBr3 nanocrystals, different concentrations of PbBr2 will also affect the fluorescence intensity, thereby affecting the Cs + The sensitivity of the test. Fig. 9 (a) and Fig. 9 (b) The range of 0.01-0.05 mol / L PbBr2 solution (fixed volume 10 μL, N-methylformamide as solvent) was investigated, and it was found that the highest PL intensity could be achieved using 0.03 mol / L PbBr2 solution. + were completely converted into CsPbBr3 NCs, while higher concentrations of PbBr2 could produce some non-fluorescent CsPb2Br5 NCs, reducing the number of CsPbBr3 NCs and leading to a decrease in PL intensity.

[0104] 2.4 Adsorption isotherms and kinetics

[0105] To describe and understand the adsorption process, the Langmuir (Equation 1) and Freundlich (Equation 2) isotherm models were used to fit the adsorption data:

[0106]

[0107] In the formula, q e (μg slice -1 ) and C e (mg L -1 ) is the equilibrium state of AMP-SiO2 film on Cs + The adsorption amount and Cs in solution + The concentration of max (μg slice -1 ) is the maximum adsorption capacity, K L , K F are the Langmuir constant and the Freundlich constant, respectively, representing the adsorption amount obtained by the appropriate fitting model, and n is the heterogeneity factor. Fig.10 and Table 3. The results show that the adsorption isotherm is more consistent with the Langmuir model, and the q max The value of 389 μg / piece is close to the experimental value (323 μg / piece), indicating that AMP-SiO2 film has a strong effect on the absorption of Cs + The adsorption is uniform in a single layer.

[0108] Table 3 Adsorption isotherm parameters of Cs+ on AMP-SiO2 film

[0109]

[0110] The pseudo-first-order and second-order kinetic models were further used to study the Cs + Adsorption kinetics on AMP-SiO2 film. The pseudo-first-order (Equation 3) and second-order (Equation 4) kinetic equations are as follows:

[0111] ln(q e -q t )=lnq e -K1t (3)

[0112]

[0113] In the formula, q e and q t The AMP-SiO2 film on Cs at equilibrium state and specific time t(min) respectively + The adsorption capacity, k1(mg L -1 ) and k2(mg L -1 ) are the equilibrium rate constants in the first-order and second-order kinetic models, respectively. Fig.11 And Table 4, the analysis results show that Cs +The adsorption on AMP-SiO2 film conforms to the second-order kinetics.

[0114] Table 4Cs + Kinetic model parameters on AMP-SiO2 film

[0115]

[0116] 2.5 Method evaluation and actual sample analysis

[0117] Under the best optimized conditions, the analytical performance of the new method was investigated. Fig.12 (a), PL intensity of CsPbBr3NCs increases with the increase of Cs + Increased with increasing concentration. Fig.12 (b) shows the fluorescence intensity of Cs + Concentration 0.0005-30μgmL -1 The linear response is within the range, the linear equation is Y = 54.695x + 29.069, and the correlation coefficient (R 2 ) was 0.9960. The limit of detection (LOD) was 0.00019 μg mL -1 (S / N=3), with a low detection limit. In addition, please refer to Fig.12 (c), the linear equation is Y = 0.624x + 484.11, and the correlation coefficient (R 2 ) is 0.9934, when Cs + Concentration from 0.001 μg mL -1 Increase to 30 μg mL -1 When the PL peak moves from 483nm to 505nm, the red shift of wavelength and Cs + The increase in the concentration of Cs + Dual response sensing mode.

[0118] In order to verify the effectiveness of this method on Cs + The selectivity of K + , Na + ,Mg 2+ , Rb + , Sr. 2+ , SO4 2- , NO3 - In the presence of + See Fig.13 , when Cs +When the concentration ratio of the coexisting ions was 1:10 and 1:50, respectively, the luminescence intensity of the formed CsPbBr3 NCs remained above 90% and 85%. Since the hydration size of cesium ions in aqueous solution is similar to that of other metal ions, it will affect the hydration of ammonium phosphomolybdate to Cs + The selectivity leads to the + During ion exchange, other metal ions are used as coordination ions, reducing the + The adsorption of NH4 in ammonium phosphomolybdate reduces the adsorption effect. + It can also be used with SO4 2- , NO3 - Coordinate with Cs + Competition with ammonium phosphomolybdate also leads to the AMP-SiO2 film's coordination with Cs + However, even in the presence of competing ions, even when the concentration ratio is Cs + The adsorption capacity of cesium ions did not decrease significantly, but decreased by 13%-15%, indicating that the material has good adsorption performance for Cs + High selectivity compared to other materials (such as DB24C8E) for Cs + After enrichment, there has been a significant improvement.

[0119] To further verify the applicability of the established method, Beihai seawater and Fangchenggang seawater were selected as test samples. Please refer to Table 5 for the fluorescence method for detecting Cs in seawater. + The detection concentration was 0.037 μg mL -1 and 0.045 μg mL -1 , and the concentration measured by atomic absorption spectrometry (AAS) was 0.047 μg mL -1 and 0.052 μg mL -1 Close. + The recovery rate of spiked product is 98.20%~107.00%, the RSD is no more than 4.90%, and the relative error between the fluorescence detection result and the atomic absorption spectrometry detection result is no more than 14.89%, which has high accuracy and precision.

[0120] Table 5 Actual sample detection and spike recovery

[0121]

[0122] a: Relative error is the comparison of graphite furnace atomic absorption.

[0123] In order to evaluate the difference in performance of different batches of AMP-SiO2 films, repeated experiments within and between batches were designed. During the repeated experiments, please refer to Table 6. The relative standard deviations (RSDs) of the test results of AMP-SiO2 films within the batch (n=5) and between batches (n=5) were 1.05% and 5.00%, respectively (Table 6), indicating that the method has good repeatability, is relatively reliable and stable.

[0124] Table 6 Reproducibility test of thin film sensing materials based on AMP-SiO2

[0125]

[0126] 3. Summary

[0127] The present invention designs a mesoporous silicon film loaded with ammonium phosphomolybdate (AMP-SiO2 film) for Cs + A highly selective and sensitive Cs separation and enrichment method was developed by in situ growth of CsPbBr3 NCs in mesoporous channels. + Fluorescence detection method. AMP-SiO2 film adsorption of Cs in the adsorption environment of pH = 3 and enrichment volume 10 mL + The adsorption capacity is 343μg / piece, and the enrichment factor is as high as 62500. Its high efficiency enrichment performance comes from Cs + With NH4 in AMP + The linear range of the method based on AMP-SiO2 film is 0.0005-30μg mL -1 , LOD was 0.00019 μg mL -1 The method can detect the concentration of 0.045 μg mL in the seawater samples of Fangchenggang and Beihai. -1 and 0.037 μg mL -1 , Cs + The recoveries ranged from 98.20% to 112.14%, with relative standard deviations of 1.61-4.9%.

[0128] Compared with the prior art, the present invention designs a mesoporous silicon film loaded with ammonium phosphomolybdate to + The selective adsorption of Cs + The mesoporous silicon film loaded with ammonium phosphomolybdate of the present invention has a stronger enrichment ability and is beneficial to reduce Cs + The present invention is to enrich Cs in a mesoporous silicon film loaded with ammonium phosphomolybdate. + Conversion into CsPbBr3 NCs to build Cs + Fluorescence detection method for Cs in complex matrix samples+ Provides new technology for the detection of radionuclides.

[0129] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, and the present invention is also intended to include these modifications and modifications.

Claims

1. A method for preparing a mesoporous silicon film loaded with ammonium phosphomolybdate, characterized in that: The following steps are involved: (1) Synthesis of mesoporous silica films Mix hexadecyltrimethylammonium chloride, ethanol and n-decane in an ammonia solution, and stir at 50-70°C until transparent to form an oil-in-water emulsion; fix the polished quartz sheet in the groove of the template and immerse it in the oil-in-water emulsion; add a mixed solution of tetraethoxysilane and ethanol, stir and react at 50-70°C for 10-14h to obtain a glass slide; take out the glass slide, wash and dry it; calcine the dried glass slide at 530-570°C for 7-9h, remove the template, and obtain a mesoporous silicon film with quartz as the substrate; (2) Loading of ammonium phosphomolybdate Dissolve phosphomolybdic acid in water, immerse the mesoporous silicon film with quartz as the substrate therein, and stir evenly for 4-6 hours; add ammonium chloride and stir for 1-3 hours; take out the film product, wash and dry, and obtain the mesoporous silicon film with quartz as the substrate loaded with ammonium phosphomolybdate, that is, the mesoporous silicon film loaded with ammonium phosphomolybdate.

2. The method for preparing the mesoporous silicon film loaded with ammonium phosphomolybdate according to claim 1, characterized in that: In step (2), the mass ratio of phosphomolybdic acid to ammonium chloride is 1:

1.

3. A mesoporous silicon film loaded with ammonium phosphomolybdate, characterized in that: The film is obtained by the preparation method of the mesoporous silicon film loaded with ammonium phosphomolybdate as described in any one of claims 1 to 2.

4. A mesoporous silicon film loaded with ammonium phosphomolybdate as claimed in claim 3 in Cs + Application in adsorption.

5. A mesoporous silicon film loaded with ammonium phosphomolybdate as claimed in claim 3 in Cs + Applications in fluorescence detection.

6. Cs in a water sample + The fluorescence detection method is characterized by: The following steps are involved: S1, Cs + Adsorption Take the mesoporous silicon film loaded with ammonium phosphomolybdate as claimed in claim 3, add it to the water sample, stir and adsorb the cesium ions (Cs + ); taking out the adsorbed film, rinsing and drying; S2. In situ growth of CsPbBr3 NCs PbBr2 solution was added dropwise onto the dried film of S1 and dried; S3. Fluorescence detection The S2 film was dried and subjected to fluorescence detection.

7. Cs in the water sample according to claim 6 + The fluorescence detection method is characterized by: In S1, the adsorption time is 15-120 min.

8. Cs in the water sample according to claim 6 + The fluorescence detection method is characterized by: In S1, the pH of the water sample was adjusted to 3-6.

9. Cs in the water sample according to claim 6 + The fluorescence detection method is characterized by: In S1, the water sample volume is 10-150 ml; in S2, the concentration of PbBr2 solution is 0.03 mol / L.

10. Cs in the water sample according to claim 6 + The fluorescence detection method is characterized by: In S3, the specific method of fluorescence detection includes the following steps: Preparation of Cs + Concentration ranges from 0.0005 to 30 μg mL -1 The multiple cesium carbonate standard solutions were used as standard water samples to perform steps S1 and S2 respectively, and the fluorescence intensity of CsPbBr3 NCs was measured. + The concentration of CsPbBr3 NCs in the water sample to be tested is plotted as a standard working curve; the water sample to be tested is taken to perform steps S1 and S2, and the fluorescence intensity of CsPbBr3 NCs measured is substituted into the above standard working curve to obtain the concentration of Cs + concentration.