Preparation and grounding configuration method and system of deep charge and discharge resistant polyetherimide composite medium
By introducing long rod-shaped zinc oxide nanoparticles into the polyetherimide matrix, the PEI/ZnO composite medium is prepared and configured for grounding, which solves the quality and cost problems of deep charge and discharge protection of spacecraft, and improves the radiation resistance and lifespan. More efficient spacecraft media protection is achieved.
Patent Information
- Application Number
- CN202411351090.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-09-26
AI Technical Summary
In the existing technology, the deep charge and discharge protection of spacecraft mainly relies on the aluminum shielding layer, which increases the quality of the spacecraft and the launch cost. In addition, there is insufficient research on the anti-deep charge and discharge performance of polyetherimide dielectric, and there is a lack of effective grounding configuration methods.
Using a combination of long rod-shaped zinc oxide nanoparticles and polyetherimide matrix, by preparing PEI/ZnO composite dielectric films, sheets and special-shaped structural parts, and conducting grounding configurations in a space radiation environment, nanoparticle modules, polyetherimide Systematic approach to imine-based composite fabrication modules and ground configuration modules.
It significantly improves the dielectric properties, structural stability and radiation resistance, extends the charge and discharge cycle life, reduces the number of electrostatic discharges and discharge current peaks, reduces the thickness of the required aluminum shielding layer, and reduces the quality and cost of spacecraft launches.
Smart Images

Figure CN118852701A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to but is not limited to the technical field of spacecraft space radiation shielding, and in particular relates to a method and system for preparing and grounding a polyetherimide composite medium with deep charge and discharge resistance. Background Art
[0002] Charged particle radiation in space is an important environmental factor that seriously threatens space activities on the orbit of spacecraft. The impact of the interaction between the space radiation environment and the spacecraft on the spacecraft is called the space radiation effect. Among them, the main ones with greater impact are: total dose effect, single particle effect and charge and discharge effect. Among them, the deep charge and discharge effect of the dielectric under the action of high-energy electrons is the most serious. Deep dielectric charge and discharge refers to high-energy electrons (0.1-10MeV) penetrating the shielding layer and the surface of the dielectric and depositing inside the dielectric. Due to the high resistivity of the insulating material, its charge release rate is much smaller than the charge deposition rate, so the charge inside the dielectric continues to accumulate, resulting in local electric field concentration. When the electric field generated by the deposited charge exceeds the breakdown threshold of the material, electrostatic discharge will occur. Deep charge and discharge of spacecraft dielectrics will cause the deterioration of the insulating dielectric and even insulation failure; at the same time, the electromagnetic pulses generated by electrostatic discharge will cause abnormal operation of the spacecraft electronic equipment. In severe cases, it will directly cause the breakdown of sensitive electronic devices of the spacecraft, threatening the safe operation of the spacecraft.
[0003] At present, the deep charge and discharge protection of aerospace dielectrics is mainly achieved by adding a shielding layer. The shielding layer material is generally aluminum. The protection of the aluminum plate can prevent or reduce high-energy electrons from entering the interior of the spacecraft dielectric material, which mainly depends on the thickness of the aluminum shielding layer. Generally, it is necessary to determine the high-energy electron energy spectrum and the corresponding electron flux according to the actual orbit of the spacecraft, and then determine the optimal thickness of the aluminum shielding layer through simulation calculation, so as to achieve the protection of deep charge and discharge of the dielectric. The disadvantage of this method is that the aluminum shielding layer is set outside the spacecraft, which will increase the overall mass of the spacecraft, resulting in a sharp increase in the launch cost; in addition, for thick insulating dielectrics (such as centimeters), the accumulated charge inside is not easy to release, and it is easy to cause dielectric charge and discharge at a lower charge density. Therefore, the required aluminum shielding thickness is greater, which further increases the launch mass of the spacecraft. On the other hand, with the development of high-voltage and high-power spacecraft, the required insulating dielectric thickness is also increasing, so it is urgent to develop new dielectric deep charge and discharge protection methods.
[0004] Polyetherimide (PEI) is a spacecraft dielectric material with excellent performance. It maintains the excellent high temperature resistance and thermal stability of polyimide (PI). PEI also has excellent mechanical properties, chemical stability, outstanding flame retardancy and low smoke density. At the same time, it has excellent electrical properties, extremely high dielectric strength and radiation resistance. It is precisely because of its excellent insulation properties that the conductivity is 5.0×10 -18 At the S / m level, the charges deposited inside it are not easy to release under electron radiation, and it is more likely to cause charge accumulation, thereby triggering deep charge and discharge phenomena in the dielectric. At present, the improvement research on polyetherimide dielectrics is mostly focused on its mechanical, friction and dielectric properties, and there is little research on its resistance to deep charge and discharge under electron radiation.
[0005] The prior art has the following technical problems: (1) Currently, deep charge and discharge protection for aerospace media is mainly achieved by adding an aluminum shielding layer. This method will increase the overall mass of the spacecraft, thereby causing a sharp increase in launch costs.
[0006] (2) With the development of high-voltage and high-power spacecraft, the required thickness of insulating media is also increasing. For thick insulating media (such as centimeter-level), the charges accumulated inside are not easy to release. Under low deposited charge density, it is easy to cause dielectric charging and discharging. If traditional aluminum shielding is used, the required shielding aluminum plate thickness is even greater, further increasing the launch mass of the spacecraft.
[0007] (3) Currently, there is little research on the deep charge and discharge protection of polyetherimide dielectrics, and there is no feasible method to improve the deep charge and discharge resistance of polyetherimide dielectrics.
[0008] (4) The grounding configuration of the dielectric is crucial in the deep charge and discharge protection of the dielectric. The current method does not provide a clear grounding configuration method for polyetherimide dielectrics. Summary of the invention
[0009] In view of the problems existing in the prior art, the present invention provides a method and system for preparing and grounding a polyetherimide composite medium with deep charge and discharge resistance.
[0010] The present invention is achieved by a method for preparing a polyetherimide composite medium having deep charge and discharge resistance and a grounding configuration method, the method comprising: S1: Preparation of long rod-shaped zinc oxide nanoparticles.
[0011] S2: Preparation of polyetherimide-based composite film specimens, polyetherimide-based composite sheet specimens, and polyetherimide-based composite special-shaped structural parts.
[0012] S3: The sample is used in the grounding configuration in a space radiation environment.
[0013] Further, the S1 specifically includes: (1) Use an electronic balance to weigh an appropriate amount of zinc nitrate hexahydrate and place it in beaker 1; then weigh a corresponding amount of sodium hydroxide and place it in beaker 1, wherein the molar ratio of zinc nitrate hexahydrate to sodium hydroxide is 1:15; add an appropriate amount of deionized water to beaker 1; stir magnetically at room temperature for 30 minutes to obtain a clear and transparent solution, and measure the pH value of the solution.
[0014] (2) The above solution was transferred to a stainless steel reactor lined with polytetrafluoroethylene, sealed, and reacted in an oven at 150°C for 8 h.
[0015] (3) Take out the above reaction kettle and cool it naturally to room temperature. Filter the solution in the reaction kettle to obtain a white precipitate; wash it with deionized water and anhydrous ethanol several times respectively, then transfer the white precipitate to a watch glass and place it in an oven at 80°C to dry for 10 hours to obtain and collect the product.
[0016] Further, in S2, preparing a polyetherimide-based composite film sample specifically includes: The PEI / ZnO composite dielectric film was prepared by blade coating and hot pressing annealing.
[0017] Raw materials and reagents: Polyetherimide (PEI) particles, SABIC-Saudi Basic Industries Corporation, Ultem1000, density 1.27g / cm 3 , Tg217°; 1-methyl-2-pyrrolidone (NMP), analytical grade, Sinopharm Chemical Reagent Co., Ltd.; long rod-shaped zinc oxide nanopowder, homemade.
[0018] The specific process is as follows: (1) Take an appropriate amount of PEI particles to be processed and homemade long rod-shaped zinc oxide powder and place them in a convection oven at 150°C and dry them for 10 hours.
[0019] (2) Weigh the corresponding mass of homemade long rod-shaped zinc oxide powder according to the set volume fraction and put it into a beaker containing 50 mL of NMP solution; place the beaker in an ultrasonic machine and oscillate it for 40 minutes until the zinc oxide powder is evenly dispersed in the NMP solution.
[0020] (3) Weigh the corresponding mass of PEI particles on a balance and add them to the dispersed mixed solution. Place the beaker on a magnetic stirrer, heat it in an oil bath and keep it at 60°C for 12 hours until the PEI particles are completely dissolved in the mixed solution. Then place the beaker containing the mixed solution in a vacuum drying oven and let it stand for 12 hours until there are no bubbles in the solution.
[0021] (4) Take out the mixed solution after standing, pour it on a clean glass substrate that has been preheated to 60°, use a film-laying scraper to evenly coat the mixed solution on the glass plate, place the glass plate in a vacuum oven at 60°C for 12 hours, then heat it to 220°C and keep it for 4 hours to remove the NMP solvent. After natural cooling, perform a film stripping treatment in deionized water to obtain the prepared PEI / ZnO composite dielectric film.
[0022] (5) After the prepared film is dried, it is heat treated in a vacuum oven to remove residual solvent, specifically, the temperature is first raised to 120°C and maintained for 5 h, then raised to 200°C and maintained for 6 h, and finally naturally cooled to room temperature.
[0023] Further, in S2, preparing a polyetherimide-based composite material sheet sample specifically comprises: The preparation is carried out by direct melt blending. The melt blending method utilizes the solubility of PEI, heats it to above its viscosity flow temperature, and then utilizes a twin-screw extruder, a twin-roll mill, a closed mixer and other mixing equipment to fully blend the polymer matrix and the filler, and finally obtains a composite material by cooling, granulating or crushing. With the help of the strong shear force of the mixing equipment, the polymer in the molten state can be well mixed with the filler to obtain a composite material.
[0024] (1) Take an appropriate amount of PEI particles to be processed and homemade long rod-shaped zinc oxide powder and place them in a convection oven at 150°C and dry them for 10 hours.
[0025] (2) Use a balance to weigh the corresponding mass of dried PEI particles and long rod-shaped zinc oxide powder according to the set ratio, mix them and set aside.
[0026] (3) Use a small laboratory closed mixer, set the mixing temperature, rotor speed, mixing time and other parameters, and then start heating.
[0027] (4) After the mixer reaches the set temperature, start the rotor and add the prepared PEI / zinc oxide mixture.
[0028] (5) After the mixing is completed, take out the mixed material and use a flat plate vulcanizer to press the mixed material into a thin sheet sample of the required size.
[0029] Further, in S2, preparing a polyetherimide-based composite material special-shaped structural member specifically comprises: (1) Take an appropriate amount of PEI particles to be processed and homemade long rod-shaped zinc oxide powder and place them in a convection oven at 150°C and dry them for 10 hours.
[0030] (2) Use a balance to weigh the corresponding mass of dried PEI particles and long rod-shaped zinc oxide powder according to the set ratio, mix them and set aside.
[0031] (3) Use a small laboratory closed mixer, set the mixing temperature, rotor speed, mixing time and other parameters, and then start heating.
[0032] (4) After the mixer reaches the set temperature, start the rotor and add the prepared PEI / zinc oxide mixture.
[0033] (5) After the mixing is completed, the mixed material is taken out and then the required special-shaped structural parts are prepared by mold casting method.
[0034] Further, the S3 specifically includes: (1) Grounding configuration method for film or sheet specimens.
[0035] Sample grounding configuration method: Film or sheet samples need to be copper plated or copper foil pasted on one side of the sample first, leaving a 3mm margin at the edge of the sample; at the same time, a special wire is used for grounding.
[0036] The special conductor consists of two copper foil patches with conductive glue and a braided copper conductor. The size of the copper foil patch is set according to the area of the copper-plated side of the film or sheet sample, generally set to 1 / 4 of its area; the length of the braided copper conductor is cut according to the actual application scenario and assembled with the copper foil patch. After assembly, one copper foil patch is attached to the center of the sample, and the copper foil patch at the other end is fixed to the grounding point. Then a multimeter is used to measure the resistance at both ends to ensure reliable grounding.
[0037] (2) Grounding configuration method for special-shaped structural parts.
[0038] Special-shaped structural parts need to be configured according to the actual installation location and purpose. For structural parts that only play a supporting role, the grounding configuration method of film or sheet-like specimens should be referred to. Copper foil should be pasted at the position where it is convenient to paste copper foil, and reliably grounded through special wires. For structural parts that play an insulating and supporting role, the insulation performance of the structural parts should be considered first. On the basis of not affecting the insulation performance of the structural parts, copper foil should be pasted at the position where it is convenient to paste copper foil on the grounding side, and reliably grounded through special wires.
[0039] Another object of the present invention is to provide a polyetherimide composite medium preparation and grounding configuration system with deep charge and discharge resistance performance based on the polyetherimide composite medium preparation and grounding configuration method with deep charge and discharge resistance performance, the system comprising: Nanoparticle module for preparing long rod-shaped zinc oxide nanoparticles.
[0040] The polyetherimide-based composite material preparation module is connected to the nanoparticle module and is used for preparing polyetherimide-based composite material film samples, polyetherimide-based composite material sheet samples, and polyetherimide-based composite material special-shaped structural parts.
[0041] The grounding configuration module is connected to the polyetherimide-based composite material preparation module, and the sample is applied to the grounding configuration in the space radiation environment.
[0042] In combination with the above technical solutions and the technical problems solved, the advantages and positive effects of the technical solutions to be protected by the present invention are as follows: First, in the prior art, polymer composite materials often show problems such as decreased dielectric properties, poor structural stability, and insufficient radiation resistance under deep charge and discharge and high radiation environments. These problems limit the application of materials in high-performance electronic components and harsh environments. For example, traditional polymer matrix materials are prone to increased dielectric loss, reduced mechanical strength, and material aging in high electric fields, high temperatures, or radiation environments, resulting in decreased system reliability. At the same time, during deep charge and discharge cycles, existing materials are also prone to dielectric degradation, charge accumulation, and other phenomena, further affecting their performance and lifespan.
[0043] 1. Improve dielectric properties.
[0044] The present invention forms a composite dielectric material by uniformly dispersing long rod-shaped zinc oxide nanoparticles in a polyetherimide (PEI) matrix. The introduction of zinc oxide nanoparticles significantly improves the dielectric constant and electrical strength of the composite material, allowing it to maintain low dielectric loss under high electric fields. This improvement enables the composite material to exhibit more stable electrical properties in high-performance electronic components and is suitable for a wider range of industrial application scenarios.
[0045] 2. Enhance structural stability.
[0046] The composite material of the present invention exhibits excellent mechanical properties under high temperature and high pressure conditions by using processes such as melt blending and mold casting. The tensile strength, impact resistance and structural integrity of the material are significantly improved, enabling it to remain stable for a long time in harsh environments. This progress expands the application of the material in aerospace, military equipment and high-demand industrial fields.
[0047] 3. Improve radiation resistance.
[0048] -The zinc oxide nanoparticles in the present invention not only improve the dielectric properties of the material, but also significantly enhance the radiation resistance of the composite material. In the space radiation environment, the material can effectively resist the impact of high-energy particles and avoid performance degradation and material aging caused by radiation. This feature makes the material of the present invention particularly suitable for aerospace and military electronic equipment to resist harsh radiation environments.
[0049] 4. Improve the performance of anti-deep charge and discharge.
[0050] - The application of the composite material of the present invention in the grounded configuration significantly improves the safety and durability of the system. The material exhibits excellent resistance to electrical aging during deep charge and discharge processes, avoiding problems such as charge accumulation and dielectric degradation. By extending the charge and discharge cycle life, the material of the present invention can effectively reduce maintenance costs and improve the overall operating efficiency of the equipment.
[0051] The present invention not only solves many key problems in the prior art by introducing long rod-shaped zinc oxide nanoparticles into the polyetherimide matrix, but also achieves significant technical progress in dielectric properties, structural stability, radiation resistance, and deep charge and discharge resistance. These advances make the material of the present invention have a wide range of application prospects in high-demand industrial applications and extreme environments.
[0052] From the results we can see: (1) Under the same radiation conditions and within the same radiation time, the number of electrostatic discharges and the peak value of discharge current of the prepared PEI / ZnO composite samples are both smaller than those of the unmodified PEI pure sample.
[0053] (2) When the electron beam current is 5 μA, compared with the pure PEI sample, the number of electrostatic discharges of the PEI / ZnO composite sample prepared by the present invention is reduced by 103 times, with a decrease of up to 89.6%.
[0054] (3) When the electron beam current is 10 μA, compared with the pure PEI sample, the number of electrostatic discharges of the PEI / ZnO composite sample prepared by the present invention is reduced by 232 times, with a decrease of up to 88.2%, which fully proves that the PEI / ZnO composite sample prepared by the present invention has excellent resistance to deep charge and discharge.
[0055] Second, the expected benefits and commercial value after the technical solution of the present invention is as follows: The present invention provides a feasible method for improving the deep charge and discharge resistance of PEI media. The prepared PEI / ZnO composite sample has significantly reduced the number of electrostatic discharges compared to the pure PEI sample under the same radiation environment, and the discharge current amplitude is also significantly reduced, which has excellent deep charge and discharge resistance. The technical solution proposed by the present invention can be applied to the deep charge and discharge protection of spacecraft media, which can effectively reduce the required aluminum shielding layer thickness, reduce the launch quality of spacecraft, and reduce the launch cost. It has excellent commercial value and good expected benefits.
[0056] The technical solution of the present invention fills the technical gap in the industry at home and abroad: starting from the spacecraft medium body, the present invention improves its deep charge and discharge resistance by doping and modifying the medium body, especially for PEI medium, which has not been studied at present. The present invention takes a different approach and provides a new route for deep charge and discharge protection of spacecraft medium, which is innovative and strong.
[0057] Third, the technical problems solved by the parameters of the present invention and the technical progress.
[0058] parameter: 1. Preparation parameters of zinc oxide nanoparticles: The molar ratio of zinc nitrate hexahydrate to sodium hydroxide is 1:15.
[0059] The reaction was carried out at 150°C for 8 hours.
[0060] The drying temperature is 80°C and the time is 10 hours.
[0061] 2. Preparation parameters of polyetherimide-based composite film: The PEI particles and the long rod-shaped zinc oxide powder were dried at 150 °C for 10 h.
[0062] The stirring temperature was 60°C and the stirring time was 12 hours.
[0063] The coating temperature was 60°C, the vacuum oven temperature was 220°C, and the temperature was kept at this temperature for 4 hours.
[0064] Heat treatment process: 120℃ for 5 hours, 200℃ for 6 hours.
[0065] 3. Preparation parameters of polyetherimide-based composite sheets and special-shaped structural parts: PEI and long rod-shaped zinc oxide powder were dried at 150 °C for 10 h.
[0066] The mixing temperature, rotor speed and time are set according to the material properties (the specific parameters depend on the actual equipment and materials).
[0067] The mold casting method is used for the molding of special-shaped structural parts.
[0068] Technical issues solved: The polymer composite materials in the prior art often face problems such as decreased dielectric properties, poor structural stability and insufficient radiation resistance under deep charge and discharge and high radiation environments. The present invention introduces long rod-shaped zinc oxide nanoparticles into the polyetherimide (PEI) matrix, which significantly improves the deep charge and discharge resistance and radiation resistance of the composite material, and solves the reliability problem of the material when used in harsh environments.
[0069] Significant technological advancements: 1. Improve dielectric properties.
[0070] The invention introduces long rod-shaped zinc oxide nanoparticles and utilizes their high dielectric constant and good dispersibility to significantly improve the dielectric properties of the polyetherimide-based composite material. In particular, under high electric field and high temperature conditions, the material can maintain a stable dielectric constant and low dielectric loss, and is suitable for high-performance electronic components.
[0071] 2. Enhance structural stability.
[0072] Composite sheets and special-shaped structural parts prepared by melt blending and mold casting have uniform structure and excellent mechanical properties, and can still maintain good structural stability under high temperature and high pressure environment. The mechanical strength and impact resistance of the material are significantly improved, making it suitable for rigorous engineering applications.
[0073] 3. Improve radiation resistance.
[0074] By introducing zinc oxide nanoparticles into the polymer matrix, the composite material of the present invention exhibits excellent radiation resistance, especially in the space radiation environment, the material can effectively resist the impact of high-energy particles and keep the electrical and physical properties of the material unaffected. This progress makes it have broad application prospects in the fields of aerospace, military electronic equipment, etc.
[0075] 4. Resistance to deep charge and discharge.
[0076] The composite material prepared by the present invention can be applied in a grounded configuration to significantly improve the safety and stability of the system. The material exhibits good resistance to electrical aging in deep charge and discharge cycles, avoiding the performance degradation problem caused by charge accumulation and dielectric degradation, and extending the service life of the equipment. BRIEF DESCRIPTION OF THE DRAWINGS
[0077] Figure 1 The present invention provides a flow chart of a method for preparing a polyetherimide composite medium with deep charge and discharge resistance and a grounding configuration method.
[0078] Figure 2 It is a grounding configuration diagram of a film or sheet sample provided in an embodiment of the present invention.
[0079] Figure 3 This is a diagram of a special conductor structure provided by an embodiment of the present invention.
[0080] Figure 4 This is a grounding configuration diagram of a thin sheet PEI / ZnO composite sample provided in an embodiment of the present invention.
[0081] Figure 5 The present invention provides a wiring diagram for a high energy electron radiation test.
[0082] Figure 6 The present invention provides a PEI / ZnO composite sample in a sheet form with grounding configuration completed. DETAILED DESCRIPTION
[0083] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0084] like Figure 1 As shown, an embodiment of the present invention provides a method for preparing a polyetherimide composite medium with deep charge and discharge resistance and grounding configuration, the method comprising: S1: Preparation of long rod-shaped zinc oxide nanoparticles.
[0085] S2: Preparation of polyetherimide-based composite film specimens, polyetherimide-based composite sheet specimens, and polyetherimide-based composite special-shaped structural parts.
[0086] S3: The sample is used in the grounding configuration in a space radiation environment.
[0087] The S1 specifically includes: (1) Use an electronic balance to weigh an appropriate amount of zinc nitrate hexahydrate and place it in beaker 1; then weigh a corresponding amount of sodium hydroxide and place it in beaker 1, wherein the molar ratio of zinc nitrate hexahydrate to sodium hydroxide is 1:15; add an appropriate amount of deionized water to beaker 1; stir magnetically at room temperature for 30 minutes to obtain a clear and transparent solution, and measure the pH value of the solution.
[0088] (2) The above solution was transferred to a stainless steel reactor lined with polytetrafluoroethylene, sealed, and reacted in an oven at 150°C for 8 h.
[0089] (3) Take out the above reaction kettle and cool it naturally to room temperature. Filter the solution in the reaction kettle to obtain a white precipitate; wash it with deionized water and anhydrous ethanol several times respectively, then transfer the white precipitate to a watch glass and place it in an oven at 80°C to dry for 10 hours to obtain and collect the product.
[0090] In S2, preparing a polyetherimide-based composite film sample specifically includes: The PEI / ZnO composite dielectric film was prepared by blade coating and hot pressing annealing.
[0091] Raw materials and reagents: Polyetherimide (PEI) particles, SABIC-Saudi Basic Industries Corporation, Ultem1000, density 1.27g / cm 3, Tg217°; 1-methyl-2-pyrrolidone (NMP), analytical grade, Sinopharm Chemical Reagent Co., Ltd.; long rod-shaped zinc oxide nanopowder, homemade.
[0092] The specific process is as follows: (1) Take an appropriate amount of PEI particles to be processed and homemade long rod-shaped zinc oxide powder and place them in a convection oven at 150°C and dry them for 10 hours.
[0093] (2) Weigh the corresponding mass of homemade long rod-shaped zinc oxide powder according to the set volume fraction and put it into a beaker containing 50 mL of NMP solution; place the beaker in an ultrasonic machine and oscillate it for 40 minutes until the zinc oxide powder is evenly dispersed in the NMP solution.
[0094] (3) Weigh the corresponding mass of PEI particles on a balance and add them to the dispersed mixed solution. Place the beaker on a magnetic stirrer, heat it in an oil bath and keep it at 60°C for 12 hours until the PEI particles are completely dissolved in the mixed solution. Then place the beaker containing the mixed solution in a vacuum drying oven and let it stand for 12 hours until there are no bubbles in the solution.
[0095] (4) Take out the mixed solution after standing, pour it on a clean glass substrate that has been preheated to 60°, use a film-laying scraper to evenly coat the mixed solution on the glass plate, place the glass plate in a vacuum oven at 60°C for 12 hours, then heat it to 220°C and keep it for 4 hours to remove the NMP solvent. After natural cooling, perform a film stripping treatment in deionized water to obtain the prepared PEI / ZnO composite dielectric film.
[0096] (5) After the prepared film is dried, it is heat treated in a vacuum oven to remove residual solvent, specifically, the temperature is first raised to 120°C and maintained for 5 h, then raised to 200°C and maintained for 6 h, and finally naturally cooled to room temperature.
[0097] In S2, preparing a polyetherimide-based composite material sheet sample specifically includes: The preparation is carried out by direct melt blending. The melt blending method utilizes the solubility of PEI, heats it to above its viscosity flow temperature, and then utilizes a twin-screw extruder, a twin-roll mill, a closed mixer and other mixing equipment to fully blend the polymer matrix and the filler, and finally obtains a composite material by cooling, granulating or crushing. With the help of the strong shear force of the mixing equipment, the polymer in the molten state can be well mixed with the filler to obtain a composite material.
[0098] (1) Take an appropriate amount of PEI particles to be processed and homemade long rod-shaped zinc oxide powder and place them in a convection oven at 150°C and dry them for 10 hours.
[0099] (2) Use a balance to weigh the corresponding mass of dried PEI particles and long rod-shaped zinc oxide powder according to the set ratio, mix them and set aside.
[0100] (3) Use a small laboratory closed mixer, set the mixing temperature, rotor speed, mixing time and other parameters, and then start heating.
[0101] (4) After the mixer reaches the set temperature, start the rotor and add the prepared PEI / zinc oxide mixture.
[0102] (5) After the mixing is completed, take out the mixed material and use a flat plate vulcanizer to press the mixed material into a thin sheet sample of the required size.
[0103] In S2, preparing a polyetherimide-based composite material special-shaped structural member specifically includes: (1) Take an appropriate amount of PEI particles to be processed and homemade long rod-shaped zinc oxide powder and place them in a convection oven at 150°C and dry them for 10 hours.
[0104] (2) Use a balance to weigh the corresponding mass of dried PEI particles and long rod-shaped zinc oxide powder according to the set ratio, mix them and set aside.
[0105] (3) Use a small laboratory closed mixer, set the mixing temperature, rotor speed, mixing time and other parameters, and then start heating.
[0106] (4) After the mixer reaches the set temperature, start the rotor and add the prepared PEI / zinc oxide mixture.
[0107] (5) After the mixing is completed, the mixed material is taken out and then the required special-shaped structural parts are prepared by mold casting method.
[0108] The S3 specifically includes: (1) Grounding configuration method for film or sheet specimens.
[0109] Sample grounding configuration method: Film or sheet samples need to be copper plated or copper foil pasted on one side of the sample, leaving a 3mm margin at the edge of the sample; Figure 2 As shown, a special wire is used for grounding; the structure of the special wire is as follows Figure 3 shown.
[0110] The special conductor consists of two copper foil patches with conductive glue and a braided copper conductor. The size of the copper foil patch is set according to the area of the copper-plated side of the film or sheet sample, generally set to 1 / 4 of its area; the length of the braided copper conductor is cut according to the actual application scenario and assembled with the copper foil patch. After assembly, one copper foil patch is attached to the center of the sample, and the copper foil patch at the other end is fixed to the grounding point. Then a multimeter is used to measure the resistance at both ends to ensure reliable grounding.
[0111] (2) Grounding configuration method for special-shaped structural parts.
[0112] Special-shaped structural parts need to be configured according to the actual installation location and purpose. For structural parts that only play a supporting role, the grounding configuration method of film or sheet-like specimens should be referred to. Copper foil should be pasted at the position where it is convenient to paste copper foil, and reliably grounded through special wires. For structural parts that play an insulating and supporting role, the insulation performance of the structural parts should be considered first. On the basis of not affecting the insulation performance of the structural parts, copper foil should be pasted at the position where it is convenient to paste copper foil on the grounding side, and reliably grounded through special wires.
[0113] The embodiment of the present invention provides a polyetherimide composite medium preparation and grounding configuration system with deep charge and discharge resistance performance based on the polyetherimide composite medium preparation and grounding configuration method with deep charge and discharge resistance performance, the system comprising: Nanoparticle module for preparing long rod-shaped zinc oxide nanoparticles.
[0114] The polyetherimide-based composite material preparation module is connected to the nanoparticle module and is used for preparing polyetherimide-based composite material film samples, polyetherimide-based composite material sheet samples, and polyetherimide-based composite material special-shaped structural parts.
[0115] The grounding configuration module is connected to the polyetherimide-based composite material preparation module, and the sample is applied to the grounding configuration in the space radiation environment.
[0116] The present invention takes a PEI / ZnO composite material in a sheet form as an example to describe in detail its preparation process and grounding configuration.
[0117] 1.1. Preparation of long rod-shaped zinc oxide nanoparticles.
[0118] (1) Use an electronic balance to weigh 5.9496 g (0.02 mol) of zinc nitrate hexahydrate and place it in a 100 mL beaker 1; then weigh 11.9991 g (0.30 mol) of sodium hydroxide and place it in beaker 1; the molar ratio of zinc nitrate hexahydrate to sodium hydroxide is 1:15; add 50 mL of deionized water to beaker 1; stir magnetically at room temperature for 30 min to obtain a clear and transparent solution, and measure the pH value of the solution.
[0119] (2) The above solution was transferred to a 100 mL polytetrafluoroethylene-lined stainless steel reactor, sealed, and reacted in an oven at 150 °C for 8 h.
[0120] (3) Take out the above reaction kettle and cool it naturally to room temperature. Filter the solution in the reaction kettle to obtain a white precipitate; wash it with deionized water and anhydrous ethanol several times respectively, then transfer the white precipitate to a watch glass and place it in an oven at 80°C to dry for 10 hours to obtain and collect the product.
[0121] (4) Repeat the above preparation process and collect a total of 100 g of product for later use.
[0122] 1.2. Prepare PEI / ZnO composite material thin film samples.
[0123] (1) Take 500 g of PEI particles, wash them several times with deionized water and anhydrous ethanol, dry them, and then place them in a convection oven at 150°C for 10 hours; take 50 g of homemade long rod-shaped zinc oxide powder and place it in a convection oven at 150°C for 10 hours.
[0124] (2) Pour the dried PEI particles and long rod-shaped zinc oxide powder into a beaker and pre-mix them. Stir them evenly with a glass rod and set aside.
[0125] (3) Use a small laboratory closed mixer for mixing, set the mixing temperature to 300°C, the rotor speed to 60 rpm, the mixing time to 15 min, and then start heating.
[0126] (4) After the mixer reaches the set temperature, start the rotor and add the prepared PEI / zinc oxide mixture.
[0127] (5) After the mixing is completed, take out the mixed material and use a flat vulcanizer to press the mixed material into a thin sheet sample of the required size. In this example, it is pressed into a circular sample with a thickness of 1 mm and a diameter of 100 mm.
[0128] 1.3. Prepare pure PEI sheet samples as the control group.
[0129] (1) Take 500 g of PEI particles, wash them several times with deionized water and anhydrous ethanol, dry them, and then place them in a convection oven at 150°C for 10 hours.
[0130] (2) Pour the dried PEI particles into a beaker and set aside.
[0131] (3) Use a small laboratory closed mixer for mixing, set the mixing temperature to 300°C, the rotor speed to 60 rpm, the mixing time to 15 min, and then start heating.
[0132] (4) After the mixer reaches the set temperature, start the rotor and add the prepared PEI particles.
[0133] (5) After the mixing is completed, take out the mixed material and use a flat vulcanizer to press the mixed material into a thin sheet sample of the required size. In this example, it is pressed into a circular sample with a thickness of 1 mm and a diameter of 100 mm.
[0134] 1.4. Grounding configuration method.
[0135] Cover one side of the circular specimen with copper foil with conductive adhesive, leaving a 3mm margin on the edge of the specimen and leaving it blank. Figure 4 As shown; at the same time, a special wire is used for grounding, and the structure of the special wire is as follows Figure 3 shown.
[0136] like Figure 4 As shown, the special conductor consists of two copper foil patches with conductive glue and a section of braided copper wire. The two copper foil patches are round with a diameter of 25 mm. Copper foil patch 1 is pasted on the center of the sample, and copper foil patch 2 is pasted and fixed on the grounding surface. After installation, a multimeter is used to measure the resistance at both ends to ensure reliable connection and good grounding.
[0137] The prepared PEI / ZnO composite sheet samples and pure PEI sheet samples were processed according to the above-mentioned grounding configuration method.
[0138] 1.5. Dielectric charge and discharge performance test.
[0139] In order to verify the deep charge and discharge resistance of the prepared PEI / ZnO sample, a high-energy electron radiation test chamber was used to conduct a comparative radiation experiment on the PEI / ZnO composite sample and the PEI pure sample under the same radiation conditions. The deep charge and discharge resistance of the sample was directly characterized by measuring the number of electrostatic discharges of each sample under electron radiation. Figure 5 shown.
[0140] Radiation test wiring diagram Figure 5 As shown, the sample is placed in a vacuum test chamber with a vacuum degree of <5×10 -4 Pa, the high-energy electron gun is placed just above the working plane, and the electrons are incident from top to bottom. The parameters of the high-energy electron generator are: electron beam current 0.2~100μA, initial electron energy: 0.3~0.5MeV, ultimate vacuum 1×10 -6 Pa.
[0141] The working platform below the radiation source is a grounded copper plate with a size of 470mm×350mm. Above the copper plate is a columnar platform made of polytetrafluoroethylene, and the test sample is placed on this platform. The test samples are all radiated from the front and grounded from the back. The lead wires from the back of the sample are grounded through a 50Ω measuring resistor, and an oscilloscope is used to collect the voltage signal at both ends of the measuring resistor.
[0142] After the radiation starts, as the radiation time increases, electrons continue to accumulate inside the sample, and the deposited charge electric field continues to increase. When the electric field strength exceeds the breakdown threshold of the sample material, it will trigger dielectric electrostatic discharge. By measuring the voltage signal on the 50Ω resistor, the corresponding discharge waveform can be collected and the number of discharges can be recorded.
[0143] The PEI / ZnO composite sample with grounding configuration is shown in Figure 1. Figure 6 shown.
[0144] Experimental results: (1) Set the electron beam current to 5 μA and measure the electrostatic discharge waveform and discharge times of the two samples within 20 minutes after the beam current stabilizes.
[0145] (2) Set the electron beam current to 10 μA and measure the electrostatic discharge waveform and discharge times of the two samples within 20 minutes after the beam current stabilizes.
[0146] Table 1 Comparative experimental results of high-energy electron radiation of two samples
[0147] It can be seen from the results that under the same radiation conditions and within the same radiation time, the number of electrostatic discharges and the peak value of the discharge current of the prepared PEI / ZnO composite sample are both less than those of the unmodified PEI pure sample. When the electron beam current is 5μA, compared with the PEI pure sample, the number of electrostatic discharges of the PEI / ZnO composite sample prepared by the present invention is reduced by 103 times, a decrease of up to 89.6%; when the electron beam current is 10μA, compared with the PEI pure sample, the number of electrostatic discharges of the PEI / ZnO composite sample prepared by the present invention is reduced by 232 times, a decrease of up to 88.2%; it is fully proved that the PEI / ZnO composite sample prepared by the present invention has excellent resistance to deep charge and discharge.
[0148] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a polyetherimide composite medium with deep charge and discharge resistance and grounding configuration, characterized in that: The method includes: S1: Preparation of long rod-shaped ZnO nanoparticles; S2: Preparation of polyetherimide-based composite film samples, polyetherimide-based composite sheet samples, and polyetherimide-based composite special-shaped structural parts; S3: The sample is used in the grounding configuration in a space radiation environment.
2. The method for preparing and grounding a polyetherimide composite medium having deep charge and discharge resistance according to claim 1, characterized in that: The S1 specifically includes: (1) Weigh an appropriate amount of zinc nitrate hexahydrate using an electronic balance and place it in beaker 1; then weigh a corresponding amount of sodium hydroxide and place it in beaker 1, wherein the molar ratio of zinc nitrate hexahydrate to sodium hydroxide is 1:15; add an appropriate amount of deionized water to beaker 1; stir magnetically at room temperature for 30 minutes to obtain a clear and transparent solution, and measure the pH value of the solution; (2) The above solution was transferred to a stainless steel reactor lined with polytetrafluoroethylene, sealed, and reacted in an oven at 150°C for 8 h; (3) Take out the above reaction kettle and cool it naturally to room temperature. Filter the solution in the reaction kettle to obtain a white precipitate; wash it with deionized water and anhydrous ethanol several times respectively, then transfer the white precipitate to a watch glass and place it in an oven at 80°C to dry for 10 hours to obtain and collect the product.
3. The method for preparing and grounding a polyetherimide composite medium having deep charge and discharge resistance as claimed in claim 1, characterized in that: In S2, preparing a polyetherimide-based composite film sample specifically includes: The PEI / ZnO composite dielectric film was prepared by blade coating and hot pressing annealing. Raw materials and reagents: Polyetherimide (PEI) particles, SABIC-Saudi Basic Industries Corporation, Ultem1000, density 1.27g / cm 3 , Tg217°; 1-methyl-2-pyrrolidone (NMP), analytical grade, Sinopharm Chemical Reagent Co., Ltd.; long rod-shaped zinc oxide nanopowder, homemade; The specific process is as follows: (1) Take an appropriate amount of PEI particles to be processed and homemade long rod-shaped zinc oxide powder and place them in a convection oven at 150°C and dry them for 10 hours; (2) Weigh the corresponding mass of homemade long rod-shaped zinc oxide powder according to the set volume fraction and put it into a beaker containing 50 mL of NMP solution; place the beaker in an ultrasonic machine and ultrasonically vibrate for 40 minutes until the zinc oxide powder is evenly dispersed in the NMP solution; (3) Weigh the corresponding mass of PEI particles on a balance and add them to the dispersed mixed solution. Place the beaker on a magnetic stirrer, heat it in an oil bath and keep it at 60°C for 12 hours until the PEI particles are completely dissolved in the mixed solution. Then, place the beaker containing the mixed solution in a vacuum drying oven and let it stand for 12 hours until there are no bubbles in the solution. (4) Taking out the mixed solution after standing, pouring it on a clean glass substrate that has been preheated to 60°, using a film-laying scraper to evenly coat the mixed solution on the glass plate, placing the glass plate in a vacuum oven at 60°C for 12 hours, then heating it to 220°C for 4 hours to remove the NMP solvent, and after natural cooling, performing a film stripping treatment in deionized water to obtain the prepared PEI / ZnO composite dielectric film; (5) After the prepared film is dried, it is heat treated in a vacuum oven to remove residual solvent, specifically, the temperature is first raised to 120°C and maintained for 5 h, then raised to 200°C and maintained for 6 h, and finally naturally cooled to room temperature.
4. The method for preparing and grounding a polyetherimide composite medium having deep charge and discharge resistance as claimed in claim 1, characterized in that: In S2, preparing a polyetherimide-based composite material sheet sample specifically includes: The preparation is carried out by direct melt blending. The melt blending method is to utilize the solubility of PEI, heat it to above its viscosity flow temperature, and then use a twin-screw extruder, a twin-roll mill, a closed mixer and other mixing equipment to fully blend the polymer matrix and the filler, and finally cool, granulate or crush to obtain a composite material. With the help of the strong shear force of the mixing equipment, the polymer in the molten state can be well mixed with the filler to obtain a composite material; (1) Take an appropriate amount of PEI particles to be processed and homemade long rod-shaped zinc oxide powder and place them in a convection oven at 150°C and dry them for 10 hours; (2) Weigh the corresponding mass of dried PEI particles and long rod-shaped zinc oxide powder according to the set ratio using a balance, mix them and set aside; (3) Using a small laboratory closed mixer, set the mixing temperature, rotor speed, mixing time and other parameters, and then start heating; (4) After the mixer reaches the set temperature, start the rotor and add the prepared PEI / zinc oxide mixture; (5) After the mixing is completed, take out the mixed material and use a flat plate vulcanizer to press the mixed material into a thin sheet sample of the required size.
5. The method for preparing and grounding a polyetherimide composite medium having deep charge and discharge resistance as claimed in claim 1, characterized in that: In S2, preparing a polyetherimide-based composite material special-shaped structural member specifically includes: (1) Take an appropriate amount of PEI particles to be processed and homemade long rod-shaped zinc oxide powder and place them in a convection oven at 150°C and dry them for 10 hours; (2) Weigh the corresponding mass of dried PEI particles and long rod-shaped zinc oxide powder according to the set ratio using a balance, mix them and set aside; (3) Using a small laboratory closed mixer, set the mixing temperature, rotor speed, mixing time and other parameters, and then start heating; (4) After the mixer reaches the set temperature, start the rotor and add the prepared PEI / zinc oxide mixture; (5) After the mixing is completed, the mixed material is taken out and then the required special-shaped structural parts are prepared by mold casting method.
6. The method for preparing and grounding a polyetherimide composite medium having deep charge and discharge resistance as claimed in claim 1, characterized in that: The S3 specifically includes: (1) Grounding configuration method for film or sheet specimens: Sample grounding configuration method: Film or sheet samples need to be copper plated or copper foil pasted on one side of the sample, leaving a 3mm margin at the edge of the sample; at the same time, a special wire is used for grounding; The special conductor consists of two copper foil patches with conductive glue and a braided copper conductor. The size of the copper foil patch is set according to the area of the copper-plated side of the film or sheet sample, generally set to 1 / 4 of its area. The length of the braided copper conductor is cut according to the actual application scenario and assembled with the copper foil patch. After assembly, one copper foil patch is attached to the center of the sample, and the copper foil patch at the other end is fixed to the grounding point. Then a multimeter is used to measure the resistance at both ends to ensure reliable grounding. (2) Grounding configuration method for special-shaped structural parts Special-shaped structural parts need to be configured according to the actual installation location and purpose. For structural parts that only play a supporting role, the grounding configuration method of film or sheet-like specimens should be referred to. Copper foil should be pasted at the position where it is convenient to paste copper foil, and reliably grounded through special wires. For structural parts that play an insulating and supporting role, the insulation performance of the structural parts should be considered first. On the basis of not affecting the insulation performance of the structural parts, copper foil should be pasted at the position where it is convenient to paste copper foil on the grounding side, and reliably grounded through special wires.
7. A polyetherimide composite medium preparation and grounding configuration system with deep charge and discharge resistance performance based on the polyetherimide composite medium preparation and grounding configuration method with deep charge and discharge resistance performance as described in any one of claims 1 to 6, characterized in that: The system includes: Nanoparticle module, used to prepare long rod-shaped zinc oxide nanoparticles; A polyetherimide-based composite material preparation module is connected to the nanoparticle module and is used to prepare polyetherimide-based composite material film samples, polyetherimide-based composite material sheet samples, and polyetherimide-based composite material special-shaped structural parts; The grounding configuration module is connected to the polyetherimide-based composite material preparation module, and the sample is applied to the grounding configuration in the space radiation environment.
Citation Information
Patent Citations
Polyvinylidene fluoride dielectric film material doped with zinc oxide and preparation method thereof
CN101494094A
Preparation method of ZnO nanorod / nanosheet composite structure photo-anode film and photo-anode film prepared by preparation method
CN105931849A
Preparation of zinc oxide nanorod-graphene nanosheet composite
CN106596674A
Oriented zinc oxide nanorod polyvinyl alcohol composite material for energy-storage capacitor and preparation method thereof
CN108948613A
Preparation method and application of cross-linked polyetherimide-based dielectric composite film
CN111004507A