Water-based multi-fluorescent anti-counterfeiting coating and preparation method thereof
By using components such as polysiloxane-modified acrylic resin, regenerated cellulose microfibers, quantum dots and fluorescent fibers in water-based multiple fluorescent anti-counterfeiting coatings, combined with the linear arrangement of quantum dots and the triple parallel structure of fluorescent fibers, the problem is solved Traditional fluorescent anti-counterfeiting coatings have problems such as poor environmental protection, single anti-counterfeiting means, difficult construction, insufficient durability and unstable fluorescent performance. We have realized environmentally friendly, multiple anti-counterfeiting, simple construction and high-performance fluorescent coatings.
Patent Information
- Application Number
- CN202410897557.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional fluorescent anti-counterfeiting coatings have problems such as poor environmental protection, single anti-counterfeiting means, difficult construction, insufficient durability and unstable fluorescent performance. In particular, the oil-based system poses a threat to the environment and construction workers, and the durability and anti-counterfeiting effect of water-based fluorescent anti-counterfeiting coatings Not ideal.
Water-based multiple fluorescent anti-counterfeiting coatings are used, including components such as polysiloxane-modified acrylic resin, regenerated cellulose microfibers, quantum dots and fluorescent fibers. Multiple fluorescent effects and complex anti-counterfeiting patterns are formed through a specific preparation process. Quantum dots are used to form multiple fluorescent anti-counterfeiting coatings. The linear arrangement and triple parallel structure of fluorescent fibers improve the fluorescent performance and anti-counterfeiting effect.
It significantly improves the environmental protection, multiple anti-counterfeiting functions, ease of construction, durability and fluorescence performance stability, reduces production costs, extends the service life of the coating, and improves the anti-counterfeiting effect and identification difficulty.
Smart Images

Figure CN118852979A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of water-based coatings, and in particular to a water-based multi-fluorescent anti-counterfeiting coating and a preparation method thereof. Background Art
[0002] With the development of commodity economy and the enhancement of awareness of intellectual property protection, anti-counterfeiting technology is increasingly used in various fields. As an important anti-counterfeiting method, fluorescent anti-counterfeiting coatings have attracted widespread attention in the market due to their unique fluorescent effects and difficult-to-copy characteristics. Traditional fluorescent anti-counterfeiting coatings are mostly based on oily systems, which have problems such as large environmental pollution, difficult construction, and high cost. Water-based fluorescent anti-counterfeiting coatings have gradually become a research hotspot due to their advantages such as environmental protection, easy construction, and low cost.
[0003] Deficiencies in the existing technology:
[0004] Poor environmental protection: Traditional oil-based fluorescent anti-counterfeiting coatings contain a large amount of organic solvents, which pose a threat to the environment and the health of construction workers. With the increasingly stringent environmental regulations, the application of such coatings is restricted.
[0005] Single anti-counterfeiting means: Many existing fluorescent anti-counterfeiting coatings only rely on a single fluorescent effect, and the anti-counterfeiting means are single and easy to be imitated.
[0006] Difficult construction: Oil-based paints have high requirements for construction conditions, dry slowly, and are not easy to apply on wet surfaces or in humid environments, which increases construction difficulty and cost.
[0007] Insufficient durability: Some water-based fluorescent anti-counterfeiting coatings tend to fade or their fluorescent effect weakens during use, affecting their anti-counterfeiting effect and service life.
[0008] Unstable fluorescence performance: When some fluorescent substances are left for a long time or exposed to a specific environment, the fluorescence intensity decays quickly, resulting in unsatisfactory anti-counterfeiting effect.
[0009] Therefore, we proposed a water-based multi-fluorescent anti-counterfeiting coating and a preparation method thereof to solve the above problems. Summary of the invention
[0010] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a water-based multi-fluorescent anti-counterfeiting coating and a preparation method thereof.
[0011] In order to achieve the above object, the present invention adopts the following technical solutions:
[0012] A water-based multiple fluorescent anti-counterfeiting coating comprises the following components in parts by weight: 30-50 parts of polysiloxane-modified acrylic resin, 5-15 parts of regenerated cellulose microfibers, 1-10 parts of quantum dots, 1-5 parts of fluorescent fibers, 10-30 parts of water-based fluorescent pigments, 0.5-3 parts of cross-linking agents, 0.5-2 parts of dispersants, and 20-60 parts of deionized water.
[0013] As the preferred technical solution:
[0014] The water-based multi-fluorescent anti-counterfeiting coating as described above includes the following components in parts by weight: 40 parts of polysiloxane-modified acrylic resin, 7 parts of regenerated cellulose microfibers, 3 parts of quantum dots, 2 parts of fluorescent fibers, 20 parts of water-based fluorescent pigments, 2 parts of cross-linking agents, 1.5 parts of dispersants, and 40 parts of deionized water.
[0015] As described above, the aqueous multi-fluorescent anti-counterfeiting coating, the fluorescent fiber is a polymer material matrix, the polymer material matrix includes polyester, fluorescent substances are uniformly dispersed inside the fluorescent fiber, the fluorescent substances include fluorescent dyes and fluorescent pigments, the cross-linking agent is an aqueous blocked isocyanate curing agent, the dispersant is one of sodium polyacrylate and sodium dodecylbenzene sulfonate, the quantum dots are ZnS:Mn / ZnS core-shell structure quantum dots, the core is ZnS:Mn, the shell is pure ZnS, the particle size of the quantum dots is controlled between 5 and 10 nanometers, the fluorescence emission wavelength of the quantum dots is concentrated between 520 and 530 nanometers, the half-peak width is less than 30 nanometers, and the aqueous fluorescent pigment is a rhodamine B-based fluorescent pigment, and the particle size is controlled between 1 and 5 microns.
[0016] In the water-based multi-fluorescent anti-counterfeiting coating as described above, the polysiloxane-modified acrylic resin is a composite of an acrylic resin with a glycidyl group and a siloxane prepolymer with a number average molecular weight of 1000 to 2000 through copolymerization or grafting, wherein the weight ratio of the acrylic resin to the siloxane prepolymer is 20:80; the diameter of the regenerated cellulose microfibers is 0.5 to 0.8 microns, the length is 50 to 100, the ellipticity of the regenerated cellulose microfibers is less than 1.5, and the surface of the regenerated cellulose microfibers is carboxylated, and the carboxyl content reaches 2% of the total weight of the fiber.
[0017] The water-based multi-fluorescent anti-counterfeiting coating as described above, wherein the polysiloxane-modified acrylic resin contains active groups, and the active groups include hydroxyl groups and carboxyl groups;
[0018] The surface of the regenerated cellulose microfiber is treated with a surface modifier A, which is a silane coupling agent containing a hydroxyl group, an amino group or an epoxy group, and the surface modifier A forms a hydrogen bond or a covalent bond with the polysiloxane-modified acrylic resin;
[0019] The surface of the quantum dots is coated with a layer of organic ligands, the organic ligands contain carboxyl groups or amino groups, the organic ligands are compatible with the polysiloxane-modified acrylic resin, and the linear arrangement of the quantum dots is achieved through the guidance of an external magnetic field or electric field;
[0020] The fluorescent fiber has a triple parallel fluorescent fiber structure. The surface of each row of fibers is treated with different fluorescent dyes. The triple parallel fluorescent fiber structure is arranged at an angle in the coating. The angle between the nth row of fluorescent fibers and the baseline is set to \theta_n, then:
[0021] \theta_n=\theta_0+(n-1)\t imes\De l ta\theta;
[0022] Wherein, \theta_0 is the reference angle of the first row of fluorescent fibers; n is the number of rows of fluorescent fibers, counting from 1; \De l ta\theta is the angle increment between two adjacent rows of fluorescent fibers;
[0023] The surface of the pigment particles of the water-based fluorescent pigment is treated with a surface modifier B, which is a carboxylic acid grafted with polyethylene glycol, and the surface modifier B forms a strong interaction with the polysiloxane-modified acrylic resin;
[0024] The crosslinking agent is a crosslinking agent with a bifunctional group, one end of which reacts with the polysiloxane-modified acrylic resin, and the other end of which reacts with the surface modifier A to form a three-dimensional network structure.
[0025] The second aspect of the present invention provides a method for preparing a water-based multi-fluorescent anti-counterfeiting coating, comprising the following steps:
[0026] S1: Selecting an acrylic resin with a glycidyl group as the main body, mixing the acrylic resin with a siloxane prepolymer with a number average molecular weight of 1000 to 2000 in a weight ratio of 20:80, and compounding by copolymerization or grafting at a temperature of 70 to 90° C. for 2 to 4 hours to form a polysiloxane-modified acrylic resin;
[0027] S2: performing surface coating treatment on the quantum dots, selecting an organic ligand containing a carboxyl group or an amino group as the coating layer, and firmly connecting the ligand to the surface of the quantum dots through chemical bonding at a temperature of 50 to 70° C., and the reaction time is 1 to 3 hours;
[0028] S3: performing surface modification treatment on the fluorescent fiber, selecting a silane coupling agent containing a hydroxyl group, an amino group or an epoxy group as the surface modifier A, and firmly grafting the modifier on the fiber surface through a chemical reaction at a temperature of 40 to 60° C., and the reaction time is 2 to 4 hours;
[0029] S4: performing surface modification treatment on pigment particles of water-based fluorescent pigment, selecting polyethylene glycol-grafted carboxylic acid as surface modifier B, and firmly adsorbing the modifier on the surface of pigment particles by physical adsorption or chemical bonding at a temperature of 30 to 50° C., and the reaction time is 1 to 2 hours;
[0030] S5: taking the polysiloxane-modified acrylic resin as the main resin, adding an appropriate amount of deionized water for dilution to form a resin aqueous solution with a solid content of 30% to 50%;
[0031] S6: adding fluorescent particles consisting of surface-modified quantum dots, fluorescent fibers and water-based fluorescent pigments to the resin aqueous solution, and uniformly dispersing the fluorescent particles in the polysiloxane-modified acrylic resin by an ultrasonic dispersion method, wherein the ultrasonic frequency is 20 to 40 kHz and the dispersion time is 30 to 60 minutes to obtain a composite resin solution;
[0032] S7: adding a dispersant to the composite resin solution to further ensure the dispersibility and stability of the composite resin solution environment;
[0033] S8: A cross-linking agent with a bifunctional group is selected and added, one end of which reacts with the active group in the polysiloxane-modified acrylic resin, and the other end reacts with the modifier on the surface of the fluorescent particles to form a three-dimensional network structure, so that the coating forms a stable cross-linked network structure to obtain a water-based multi-fluorescent anti-counterfeiting coating.
[0034] As the preferred technical solution:
[0035] In the method for preparing a water-based multi-fluorescent anti-counterfeiting coating as described above, in S2, the linear arrangement of the quantum dots is achieved by applying an external magnetic field, the quantum dots are dispersed in a solvent to form a stable solution, an electromagnet or a permanent magnet is used to generate the required magnetic field, and the direction and intensity of the magnetic field are adjusted, and the quantum dot solution is placed in the magnetic field. Under the action of the magnetic force, the quantum dots are gradually arranged along the direction of the magnetic field to achieve linear arrangement, and the relationship between the magnetic moment of the quantum dots and the magnetic field gradient is:
[0036] F_m=\mu_0\cdotm\cdot\nab l aB;
[0037] Among them, F_m is the magnetic force on the quantum dot, \mu_0 is the magnetic permeability of the vacuum, m is the magnetic moment of the quantum dot, \nab laB is the magnetic field gradient;
[0038] Calculation of quantum dot magnetic moment:
[0039] m=n\cdot\mu_B\cdotg_J\cdotJ;
[0040] Where n is the number of magnetic ions in the quantum dot, \mu_B is the Bohr magneton, g_J is the Lande g factor, and J is the total angular momentum of the quantum dot;
[0041] Calculation of magnetic field gradient:
[0042] \nab l aB=\frac{B_2-B_1}{d};
[0043] Among them, B_2 and B_1 are the magnetic field intensities at two different positions in the direction of quantum dot arrangement, and d is the distance between the two positions.
[0044] In the method for preparing a water-based multiple fluorescent anti-counterfeiting coating as described above, in S3, the fluorescent fiber comprises a base fiber material, and the base fiber material comprises polyester fiber;
[0045] The basic fibers are woven into a triple parallel structure using textile technology, with spacing between each row of fibers. The surface of each row is treated with fluorescent dyes of different colors. A silane coupling agent containing a hydroxyl group, an amino group or an epoxy group is selected as a surface modifier. The triple parallel fluorescent fiber structure is immersed in an aqueous solution of the surface modifier, and the temperature is controlled between 40 and 60° C. The reaction is performed for 2 to 4 hours to firmly graft the modifier on the fiber surface. The triple parallel fluorescent fiber structure after surface modification is arranged at a preset angle K and added to the coating.
[0046] Using multi-layer coating technology, coatings containing fluorescent fibers arranged at different angles are applied to the substrate in sequence to form a coating with multiple fluorescent effects and complex anti-counterfeiting patterns.
[0047] The preparation method of a water-based multiple fluorescent anti-counterfeiting coating as described above, wherein S4 further includes S41: using a high-speed disperser to disperse the regenerated cellulose microfibers in deionized water, the dispersion speed is controlled at 8000-12000 rpm, the dispersion time is 10-30 minutes, to form a uniform fiber suspension, and during the dispersion process, the temperature of the suspension is controlled between 20°C and 30°C.
[0048] A method for preparing a water-based multiple fluorescent anti-counterfeiting coating as described above, in S8, at a temperature of 50 to 70°C, a cross-linking agent with a bifunctional group is selected and added, one end of the cross-linking agent reacts with the active group in the polysiloxane-modified acrylic resin, and the other end reacts with the modifier on the surface of the fluorescent particles to form a three-dimensional network structure, and the cross-linking and curing reaction time is 2 to 6 hours, so that the coating forms a stable cross-linked network structure to obtain a water-based multiple fluorescent anti-counterfeiting coating.
[0049] Compared with the prior art, the present invention is mainly composed of a variety of functional materials such as polysiloxane-modified acrylic resin, regenerated cellulose microfibers, quantum dots, fluorescent fibers, and water-based fluorescent pigments. Through a specific preparation process, a coating with multiple fluorescent effects and complex anti-counterfeiting patterns is formed. Among them, the introduction of fluorescent fibers and quantum dots gives the coating a unique fluorescent property and anti-counterfeiting effect; while the polysiloxane-modified acrylic resin provides good film-forming properties and weather resistance.
[0050] Beneficial effects:
[0051] Improved environmental performance: The use of a water-based system reduces the use of organic solvents, significantly reduces VOC emissions, is more environmentally friendly, and is in line with the development trend of modern green chemistry.
[0052] Multiple anti-counterfeiting functions: By combining a variety of functional materials, such as fluorescent fibers, quantum dots, etc., multiple fluorescent effects and complex anti-counterfeiting structures are achieved, which greatly improves the anti-counterfeiting effect and identification difficulty, and effectively prevents product counterfeiting and imitation.
[0053] Easy construction: Water-based paint is easy to apply and can be directly applied on wet surfaces and in humid environments. It has a moderate drying speed, which is convenient for large-scale promotion and application, reducing construction costs and time.
[0054] Strong durability: By optimizing the formula and preparation process, the durability and stability of the coating are improved, ensuring that the fluorescent effect lasts forever and extending the service life of the coating.
[0055] Low cost: The use of relatively low-cost raw materials and simple production processes reduces production costs, improves market competitiveness, and is conducive to the popularization and promotion of products.
[0056] Stable fluorescence performance: The use of fluorescent materials with stable fluorescence performance and optimized surface modification treatment process ensures that the fluorescence intensity remains unchanged for a long time, thereby improving the practicality and reliability of the coating.
[0057] In summary, the water-based multiple fluorescent anti-counterfeiting coating and its preparation method proposed in the present invention have multiple beneficial effects such as significant environmental protection, multiple anti-counterfeiting functions, simple construction, strong durability, low cost and stable fluorescent performance, etc., which provide new ideas and directions for the development of anti-counterfeiting technology and are expected to be widely used and promoted in many fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 It is a data line chart of the embodiments and comparative examples of the present invention;
[0059] Figure 2 It is a data bar chart of the embodiments and comparative examples of the present invention. DETAILED DESCRIPTION
[0060] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs. In the event of a conflict, the definitions in the specification shall prevail. "When mass, concentration, temperature, time, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values and lower preferred values, this should be understood to specifically disclose all ranges formed by any pairing of any upper range limit or preferred value with any lower range limit or preferred value, regardless of whether the range is disclosed separately. For example, a range of 1-50 should be understood to include 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61, 62, 63, 64, 65, 66, 67, 68, 69, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91 6, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, or 50, any number, combination of numbers, or subrange, and all decimal values between the above integers, for example, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, and 1.9. With respect to subranges, "nested subranges" extending from any endpoint within the range are specifically contemplated. For example, nested subranges of the exemplary range 1-50 may include 1-10, 1-20, 1-30, and 1-40 in one direction, or 50-40, 50-30, 50-20, and 50-10 in the other direction."
[0061] The present invention is further explained below in conjunction with specific examples. The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are all commercially available unless otherwise specified.
[0062] A water-based multiple fluorescent anti-counterfeiting coating comprises the following components in parts by weight: 30-50 parts of polysiloxane-modified acrylic resin, 5-15 parts of regenerated cellulose microfibers, 1-10 parts of quantum dots, 1-5 parts of fluorescent fibers, 10-30 parts of water-based fluorescent pigments, 0.5-3 parts of cross-linking agents, 0.5-2 parts of dispersants, and 20-60 parts of deionized water.
[0063] Among them, the fluorescent fiber is a polymer material matrix, the polymer material matrix includes polyester, fluorescent substances are uniformly dispersed in the fluorescent fiber, the fluorescent substances include fluorescent dyes and fluorescent pigments, the cross-linking agent uses a water-based blocked isocyanate curing agent, the dispersant is one of sodium polyacrylate and sodium dodecylbenzene sulfonate, the quantum dots use ZnS:Mn / ZnS core-shell structure quantum dots, the core is ZnS:Mn, the shell is pure ZnS, the particle size of the quantum dots is controlled between 5 and 10 nanometers, the fluorescence emission wavelength of the quantum dots is concentrated between 520 and 530 nanometers, the half-peak width is less than 30 nanometers, and the water-based fluorescent pigment is a rhodamine B-based fluorescent pigment with a particle size controlled between 1 and 5 microns.
[0064] Specifically, the polysiloxane-modified acrylic resin is a composite of an acrylic resin with a glycidyl group and a siloxane prepolymer with a number average molecular weight of 1000 to 2000 through copolymerization or grafting, wherein the weight ratio of the acrylic resin to the siloxane prepolymer is 20:80; the diameter of the regenerated cellulose microfibers is 0.5 to 0.8 microns, the length is 50 to 100, the ellipticity of the regenerated cellulose microfibers is less than 1.5, and the surface of the regenerated cellulose microfibers is carboxylated, and the carboxyl content reaches 2% of the total weight of the fiber.
[0065] The polysiloxane-modified acrylic resin contains active groups, including hydroxyl groups and carboxyl groups; the surface of the regenerated cellulose microfiber is treated with a surface modifier A, which is a silane coupling agent containing a hydroxyl group, an amino group or an epoxy group, and the surface modifier A forms a hydrogen bond or a covalent bond with the polysiloxane-modified acrylic resin; the surface of the quantum dots is coated with a layer of organic ligands, which contain carboxyl groups or amino groups and are compatible with the polysiloxane-modified acrylic resin, and the linear arrangement of the quantum dots is achieved by guiding an external magnetic field or an electric field;
[0066] The fluorescent fiber has a triple parallel fluorescent fiber structure. The surface of each row of fibers is treated with different fluorescent dyes. The triple parallel fluorescent fiber structure is arranged at an angle in the coating. The angle between the nth row of fluorescent fibers and the baseline is set to \theta_n, then:
[0067] \theta_n=\theta_0+(n-1)\t imes\De l ta\theta;
[0068] Wherein, \theta_0 is the reference angle of the first row of fluorescent fibers; n is the number of rows of fluorescent fibers, counting from 1; \De l ta\theta is the angle increment between two adjacent rows of fluorescent fibers;
[0069] Here, polyester fiber with good fluorescence performance and mechanical strength is selected as the basic material. Fluorescent fibers are prepared by melt spinning or solution spinning. During the spinning process, fluorescent dyes of different colors (such as red, green, and blue) are added to the spinning solution respectively, so that each row of fibers can obtain different fluorescent colors during the spinning process.
[0070] If it is necessary to further enhance the fluorescence effect or improve the compatibility of the fiber with the coating, the fluorescent fiber can be surface treated, for example, by using a silane coupling agent containing a hydroxyl group, an amino group or an epoxy group to modify the fiber surface.
[0071] A triple parallel fluorescent fiber structure is designed, in which the surface of each row of fibers presents three different fluorescent colors: red, green, and blue. The angle \θ_0 between the first row of fluorescent fibers (red) and the baseline is set to 20°. The angle increment Δ\θ between two adjacent rows of fluorescent fibers is set to 5°. According to the formula \θ_n=\θ_0+(n-1)×Δ\θ, the angle of the second row (green) fibers is calculated to be 25°, and the angle of the third row (blue) fibers is 30°.
[0072] Add the processed triple parallel fluorescent fibers to the basic formula of water-based multi-fluorescent anti-counterfeiting coating according to the designed arrangement. Use a high-speed stirrer or dispersing equipment to evenly disperse the fluorescent fibers in the coating to ensure that the fibers maintain the designed arrangement in the coating.
[0073] The surface of the pigment particles of the water-based fluorescent pigment is treated with a surface modifier B, which is a carboxylic acid grafted with polyethylene glycol. The surface modifier B forms a strong interaction with the polysiloxane-modified acrylic resin; the cross-linking agent is a cross-linking agent with a bifunctional group, one end of which reacts with the polysiloxane-modified acrylic resin and the other end reacts with the surface modifier A to form a three-dimensional network structure.
[0074] Embodiment 1
[0075] A water-based multi-fluorescent anti-counterfeiting coating comprises the following components in parts by weight: 30 parts of polysiloxane-modified acrylic resin, 5 parts of regenerated cellulose microfibers, 1 part of quantum dots, 1 part of fluorescent fibers, 10 parts of water-based fluorescent pigments, 0.5 parts of cross-linking agents, 0.5 parts of dispersants, and 20 parts of deionized water.
[0076] The embodiment also provides a method for preparing a water-based multi-fluorescent anti-counterfeiting coating, comprising the following steps:
[0077] S1: Selecting an acrylic resin with a glycidyl group as the main body, mixing the acrylic resin with a siloxane prepolymer with a number average molecular weight of 1000 in a weight ratio of 20:80, and compounding by copolymerization or grafting at a temperature of 70° C. for 2 hours to form a polysiloxane-modified acrylic resin;
[0078] S2: Surface coating of quantum dots is performed, and organic ligands containing carboxyl or amino groups are selected as coating layers. The ligands are firmly connected to the surface of quantum dots through chemical bonding at a temperature of 50°C, and the reaction time is 1 hour;
[0079] S3: Surface modification of the fluorescent fiber is performed by selecting a silane coupling agent containing a hydroxyl group, an amino group or an epoxy group as the surface modifier A. The modifier is firmly grafted onto the fiber surface through a chemical reaction at a temperature of 40°C. The reaction time is 2 hours.
[0080] S4: performing surface modification treatment on pigment particles of water-based fluorescent pigment, selecting polyethylene glycol-grafted carboxylic acid as surface modifier B, and firmly adsorbing the modifier on the surface of pigment particles by physical adsorption or chemical bonding at a temperature of 30° C., and the reaction time is 1 hour;
[0081] S41: using a high-speed disperser to disperse the regenerated cellulose microfibers in deionized water, the dispersion speed is controlled at 8000-12000 rpm, the dispersion time is 10-30 minutes, to form a uniform fiber suspension, and during the dispersion process, the temperature of the suspension is controlled between 20° C. and 30° C.;
[0082] S5: taking polysiloxane-modified acrylic resin as the main resin, adding an appropriate amount of deionized water for dilution to form a resin aqueous solution with a solid content of 30%;
[0083] S6: adding fluorescent particles consisting of surface-modified quantum dots, fluorescent fibers and water-based fluorescent pigments to the resin aqueous solution, and uniformly dispersing the fluorescent particles in the polysiloxane-modified acrylic resin by an ultrasonic dispersion method, with an ultrasonic frequency of 20 kHz and a dispersion time of 30 minutes to obtain a composite resin solution;
[0084] S7: adding a dispersant to the composite resin solution to further ensure the dispersibility and stability of the composite resin solution environment;
[0085] S8: At a temperature of 50°C, a cross-linking agent with a bifunctional group is selected and added. One end of the cross-linking agent reacts with the active group in the polysiloxane-modified acrylic resin, and the other end reacts with the modifier on the surface of the fluorescent particles to form a three-dimensional network structure. The cross-linking and curing reaction time is 2 hours, so that the coating forms a stable cross-linked network structure to obtain a water-based multi-fluorescent anti-counterfeiting coating.
[0086] Embodiment 2
[0087] A water-based multiple fluorescent anti-counterfeiting coating comprises the following components in parts by weight: 35 parts of polysiloxane-modified acrylic resin, 7 parts of regenerated cellulose microfibers, 3 parts of quantum dots, 2 parts of fluorescent fibers, 15 parts of water-based fluorescent pigments, 1.5 parts of cross-linking agents, 0.8 parts of dispersants, and 30 parts of deionized water.
[0088] The embodiment also provides a method for preparing a water-based multi-fluorescent anti-counterfeiting coating, comprising the following steps:
[0089] S1: Selecting an acrylic resin with a glycidyl group as the main body, mixing the acrylic resin with a siloxane prepolymer with a number average molecular weight of 1500 in a weight ratio of 20:80, and compounding by copolymerization or grafting at a temperature of 80° C. for 3 hours to form a polysiloxane-modified acrylic resin;
[0090] S2: Surface coating of quantum dots is performed, and organic ligands containing carboxyl or amino groups are selected as coating layers. The ligands are firmly connected to the surface of quantum dots through chemical bonding at a temperature of 55°C, and the reaction time is 2 hours;
[0091] S3: Surface modification of the fluorescent fiber is performed by selecting a silane coupling agent containing a hydroxyl group, an amino group or an epoxy group as the surface modifier A. The modifier is firmly grafted onto the fiber surface through a chemical reaction at a temperature of 45°C. The reaction time is 3 hours.
[0092] S4: performing surface modification treatment on pigment particles of water-based fluorescent pigment, selecting polyethylene glycol-grafted carboxylic acid as surface modifier B, and firmly adsorbing the modifier on the surface of pigment particles by physical adsorption or chemical bonding at a temperature of 35° C., and the reaction time is 1 hour;
[0093] S41: using a high-speed disperser to disperse the regenerated cellulose microfibers in deionized water, the dispersion speed is controlled at 8000-12000 rpm, the dispersion time is 10-30 minutes, to form a uniform fiber suspension, and during the dispersion process, the temperature of the suspension is controlled between 20° C. and 30° C.;
[0094] S5: taking polysiloxane-modified acrylic resin as the main resin, adding an appropriate amount of deionized water for dilution to form a resin aqueous solution with a solid content of 35%;
[0095] S6: adding fluorescent particles consisting of surface-modified quantum dots, fluorescent fibers and water-based fluorescent pigments to the resin aqueous solution, and uniformly dispersing the fluorescent particles in the polysiloxane-modified acrylic resin by an ultrasonic dispersion method, the ultrasonic frequency is 25 kHz, and the dispersion time is 40 minutes to obtain a composite resin solution;
[0096] S7: adding a dispersant to the composite resin solution to further ensure the dispersibility and stability of the composite resin solution environment;
[0097] S8: At a temperature of 55°C, a cross-linking agent with a bifunctional group is selected and added. One end of the cross-linking agent reacts with the active group in the polysiloxane-modified acrylic resin, and the other end reacts with the modifier on the surface of the fluorescent particles to form a three-dimensional network structure. The cross-linking and curing reaction time is 3 hours, so that the coating forms a stable cross-linked network structure to obtain a water-based multi-fluorescent anti-counterfeiting coating.
[0098] Embodiment 3
[0099] A water-based multiple fluorescent anti-counterfeiting coating comprises the following components in parts by weight: 40 parts of polysiloxane-modified acrylic resin, 11 parts of regenerated cellulose microfibers, 7 parts of quantum dots, 3 parts of fluorescent fibers, 20 parts of water-based fluorescent pigments, 2 parts of cross-linking agents, 1.5 parts of dispersants, and 50 parts of deionized water.
[0100] The embodiment also provides a method for preparing a water-based multi-fluorescent anti-counterfeiting coating, comprising the following steps:
[0101] S1: Selecting an acrylic resin with a glycidyl group as the main body, mixing the acrylic resin with a siloxane prepolymer with a number average molecular weight of 1800 in a weight ratio of 20:80, and compounding by copolymerization or grafting at a temperature of 80° C. for 3 hours to form a polysiloxane-modified acrylic resin;
[0102] S2: Surface coating of quantum dots is performed, and organic ligands containing carboxyl or amino groups are selected as coating layers. The ligands are firmly connected to the surface of quantum dots through chemical bonding at a temperature of 60°C, and the reaction time is 2 hours;
[0103] S3: Surface modification of the fluorescent fiber is performed by selecting a silane coupling agent containing a hydroxyl group, an amino group or an epoxy group as the surface modifier A. The modifier is firmly grafted onto the fiber surface through a chemical reaction at a temperature of 50°C. The reaction time is 3 hours.
[0104] S4: performing surface modification treatment on pigment particles of water-based fluorescent pigment, selecting polyethylene glycol-grafted carboxylic acid as surface modifier B, and firmly adsorbing the modifier on the surface of pigment particles by physical adsorption or chemical bonding at a temperature of 40° C., and the reaction time is 2 hours;
[0105] S41: using a high-speed disperser to disperse the regenerated cellulose microfibers in deionized water, the dispersion speed is controlled at 8000-12000 rpm, the dispersion time is 10-30 minutes, to form a uniform fiber suspension, and during the dispersion process, the temperature of the suspension is controlled between 20° C. and 30° C.;
[0106] S5: taking polysiloxane-modified acrylic resin as the main resin, adding an appropriate amount of deionized water for dilution to form a resin aqueous solution with a solid content of 40%;
[0107] S6: adding fluorescent particles consisting of surface-modified quantum dots, fluorescent fibers and water-based fluorescent pigments to the resin aqueous solution, and uniformly dispersing the fluorescent particles in the polysiloxane-modified acrylic resin by an ultrasonic dispersion method, with an ultrasonic frequency of 30 kHz and a dispersion time of 50 minutes to obtain a composite resin solution;
[0108] S7: adding a dispersant to the composite resin solution to further ensure the dispersibility and stability of the composite resin solution environment;
[0109] S8: At a temperature of 60°C, a cross-linking agent with a bifunctional group is selected and added. One end of the cross-linking agent reacts with the active group in the polysiloxane-modified acrylic resin, and the other end reacts with the modifier on the surface of the fluorescent particles to form a three-dimensional network structure. The cross-linking and curing reaction time is 5 hours, so that the coating forms a stable cross-linked network structure to obtain a water-based multi-fluorescent anti-counterfeiting coating.
[0110] Embodiment 4
[0111] A water-based multiple fluorescent anti-counterfeiting coating comprises the following components in parts by weight: 50 parts of polysiloxane-modified acrylic resin, 15 parts of regenerated cellulose microfibers, 10 parts of quantum dots, 5 parts of fluorescent fibers, 30 parts of water-based fluorescent pigments, 3 parts of cross-linking agents, 2 parts of dispersants, and 60 parts of deionized water.
[0112] The embodiment also provides a method for preparing a water-based multi-fluorescent anti-counterfeiting coating, comprising the following steps:
[0113] S1: Selecting an acrylic resin with a glycidyl group as the main body, mixing the acrylic resin with a siloxane prepolymer with a number average molecular weight of 2000 in a weight ratio of 20:80, and compounding by copolymerization or grafting at a temperature of 90° C. for 4 hours to form a polysiloxane-modified acrylic resin;
[0114] S2: Surface coating of quantum dots is performed, and organic ligands containing carboxyl or amino groups are selected as coating layers. The ligands are firmly connected to the surface of quantum dots through chemical bonding at a temperature of 70°C, and the reaction time is 3 hours;
[0115] S3: Surface modification of the fluorescent fiber is performed by selecting a silane coupling agent containing a hydroxyl group, an amino group or an epoxy group as the surface modifier A. The modifier is firmly grafted onto the fiber surface through a chemical reaction at a temperature of 60°C. The reaction time is 4 hours.
[0116] S4: performing surface modification treatment on pigment particles of water-based fluorescent pigment, selecting polyethylene glycol-grafted carboxylic acid as surface modifier B, and firmly adsorbing the modifier on the surface of pigment particles by physical adsorption or chemical bonding at a temperature of 50° C., and the reaction time is 2 hours;
[0117] S41: using a high-speed disperser to disperse the regenerated cellulose microfibers in deionized water, the dispersion speed is controlled at 8000-12000 rpm, the dispersion time is 10-30 minutes, to form a uniform fiber suspension, and during the dispersion process, the temperature of the suspension is controlled between 20° C. and 30° C.;
[0118] S5: taking polysiloxane-modified acrylic resin as the main resin, adding an appropriate amount of deionized water for dilution to form a resin aqueous solution with a solid content of 50%;
[0119] S6: adding fluorescent particles consisting of surface-modified quantum dots, fluorescent fibers and water-based fluorescent pigments to the resin aqueous solution, and uniformly dispersing the fluorescent particles in the polysiloxane-modified acrylic resin by an ultrasonic dispersion method, the ultrasonic frequency is 40 kHz, and the dispersion time is 60 minutes to obtain a composite resin solution;
[0120] S7: adding a dispersant to the composite resin solution to further ensure the dispersibility and stability of the composite resin solution environment;
[0121] S8: At a temperature of 70°C, a cross-linking agent with a bifunctional group is selected and added. One end of the cross-linking agent reacts with the active group in the polysiloxane-modified acrylic resin, and the other end reacts with the modifier on the surface of the fluorescent particles to form a three-dimensional network structure. The cross-linking and curing reaction time is 6 hours, so that the coating forms a stable cross-linked network structure to obtain a water-based multi-fluorescent anti-counterfeiting coating.
[0122] Comparative Example 1
[0123] A method for preparing a water-based multi-fluorescent anti-counterfeiting coating, based on Example 4, further in S2, a linear arrangement of quantum dots is achieved by applying an external magnetic field, the quantum dots are dispersed in a solvent to form a stable solution, an electromagnet or a permanent magnet is used to generate the required magnetic field, and the direction and intensity of the magnetic field are adjusted, and the quantum dot solution is placed in the magnetic field. Under the action of the magnetic force, the quantum dots are gradually arranged along the direction of the magnetic field to achieve linear arrangement, and the relationship between the magnetic moment of the quantum dots and the magnetic field gradient is:
[0124] F_m=\mu_0\cdotm\cdot\nab l aB;
[0125] Among them, F_m is the magnetic force on the quantum dot, \mu_0 is the magnetic permeability of the vacuum, m is the magnetic moment of the quantum dot, \nab laB is the magnetic field gradient;
[0126] Calculation of quantum dot magnetic moment:
[0127] m=n\cdot\mu_B\cdotg_J\cdotJ;
[0128] Where n is the number of magnetic ions in the quantum dot, \mu_B is the Bohr magneton, g_J is the Lande g factor, and J is the total angular momentum of the quantum dot;
[0129] Calculation of magnetic field gradient:
[0130] \nab l aB=\frac{B_2-B_1}{d};
[0131] Among them, B_2 and B_1 are the magnetic field intensities at two different positions in the direction of quantum dot arrangement, and d is the distance between the two positions.
[0132] The specific implementation is as follows:
[0133] Material preparation: Quantum dots: CdSe / ZnS core-shell structure, particle size 5nm, surface coated with carboxyl ligands, number of magnetic ions n=1000. Solvent: deionized water. Magnetic field generating equipment: electromagnet, magnetic field direction and intensity can be adjusted. Magnetic field measuring equipment: Gauss meter. Others: stirrer, container, etc.
[0134] Steps and operations, preparation of quantum dot solution: disperse the quantum dots in deionized water and stir with a stirrer for 30 minutes to ensure that the quantum dots are evenly dispersed. Adjust the concentration of the quantum dot solution to make it suitable for the subsequent magnetic field alignment process.
[0135] Magnetic field setting and measurement: Use an electromagnet to generate the required magnetic field, and adjust the direction and strength of the magnetic field. Select two positions in the direction of quantum dot arrangement, and use a Gauss meter to measure the magnetic field strength B_1 and B_2 at these two positions. For example, B_1 = 0.1T, B_2 = 0.2T, and the distance between the two positions d = 1cm.
[0136] Calculation of magnetic field gradient: According to the calculation formula of magnetic field gradient \nab l aB=\frac{B_2-B_1}{d}, substitute the measured values of B_1, B_2 and d to calculate the magnetic field gradient \nab l aB=10T / m.
[0137] Calculation of quantum dot magnetic moment: According to the calculation formula of quantum dot magnetic moment m=n\cdot\mu_B\cdotg_J\cdotJ, substitute the number of magnetic ions in the quantum dot n=1000, Bohr magneton \mu_B=9.274×10^-24J / T, Lande g factor g_J (assumed to be 2), and the total angular momentum of the quantum dot J (assumed to be 1 / 2), and calculate the magnetic moment m of the quantum dot.
[0138] Magnetic field arrangement of quantum dots: Place the quantum dot solution in the magnetic field generated by an electromagnet, adjust the direction and strength of the magnetic field, and gradually align the quantum dots along the direction of the magnetic field under the action of the magnetic force. During the arrangement process, the fluorescence changes of the quantum dot solution can be observed to preliminarily determine whether the quantum dots have been arranged in the expected direction.
[0139] Use appropriate detection methods (such as fluorescence microscopy, electron microscopy, etc.) to verify whether the quantum dots have achieved linear arrangement. If the arrangement effect needs to be adjusted, it can be optimized by changing parameters such as magnetic field strength, direction, or concentration of quantum dot solution.
[0140] In the second implementation of comparative example 1, the materials are prepared as follows:
[0141] Quantum dots:
[0142] Type: ZnS:Mn / ZnS core-shell structure quantum dots;
[0143] Core ingredients: ZnS:Mn;
[0144] Shell composition: pure ZnS;
[0145] Particle size range: 8 nanometers;
[0146] Fluorescence emission wavelength range: 520 nm;
[0147] Dosage: 20 g; Solvent: deionized water, dosage is 100 ml; Surfactant: select one or more surfactants suitable for water-based systems, such as sodium dodecyl sulfate (SDS), the dosage is 2% of the mass of quantum dots; Electromagnet or permanent magnet: equipment that can generate a uniform magnetic field, the magnetic field strength can be adjusted to 0.5 Tesla; Other coating ingredients: added as needed, such as film formers, thickeners, etc., the specific types and dosages refer to the conventional water-based coating formula
[0148] Linear arrangement of quantum dots, scattered quantum dots:
[0149] 20 g of ZnS:Mn / ZnS quantum dots were added into 100 ml of deionized water.
[0150] 1 g of SDS surfactant was added, and an ultrasonic disperser was used to disperse the solution at a frequency of 40 kHz for 30 minutes to form a stable quantum dot solution.
[0151] Generate a magnetic field:
[0152] Use an electromagnet or permanent magnet and adjust the magnetic field strength to 0.5 Tesla.
[0153] Ensure that the magnetic field is directed uniformly and perpendicular to the expected alignment of the quantum dot solution.
[0154] Arrangement of quantum dots:
[0155] The quantum dot solution is placed in a magnetic field and maintained for a certain period of time (such as 2 hours) so that the quantum dots are gradually arranged along the direction of the magnetic field under the action of the magnetic force.
[0156] According to the magnetic field gradient formula ((\nab la B=\frac{B_2-B_1}{d})), in this example, assuming (B_2=0.5) Tesla, (B_1=0.1) Tesla (measured at the edge of the solution), and (d=1) cm (solution thickness), then (\nab la B=40) Tesla / meter.
[0157] Through the above, the linear arrangement of quantum dots in water-based multi-fluorescent anti-counterfeiting coatings can be specifically realized, and the coatings can be given a unique fluorescent anti-counterfeiting effect.
[0158] Comparative Example 2
[0159] A method for preparing a water-based multiple fluorescent anti-counterfeiting coating, based on Example 4, in S3, the fluorescent fiber has a basic fiber material, and the basic fiber material includes polyester fiber; the basic fiber is woven into a triple parallel structure using textile technology, and a spacing is maintained between each row of fibers, and the surface of each row is treated with fluorescent dyes of different colors, and a silane coupling agent containing a hydroxyl group, an amino group or an epoxy group is selected as a surface modifier, and the triple parallel fluorescent fiber structure is immersed in an aqueous solution of the surface modifier, and the temperature is controlled between 50°C and reacted for 3 hours to firmly graft the modifier on the fiber surface, and the surface-modified triple parallel fluorescent fiber structure is added to the coating at a preset angle K; a multi-layer coating technology is used to sequentially coat the coating containing fluorescent fibers arranged at different angles on a substrate to form a coating with multiple fluorescent effects and a complex anti-counterfeiting pattern.
[0160] The details of realizing the structure of triple parallel fluorescent fibers are as follows:
[0161] Materials and equipment, basic fiber material: polyester fiber, select polyester chips with good mechanical properties and spinnability as raw materials. Fluorescent dyes: red, green and blue fluorescent dyes, ensure that each dye has a distinct fluorescent effect under ultraviolet light. Surface modifier: Silane coupling agent containing hydroxyl group, used to enhance the bonding force between fiber and coating and the fluorescent properties of fiber. Solvent: deionized water, used to prepare aqueous solution of surface modifier. Textile equipment: weaving machine, used to weave basic fibers into a triple parallel structure. Coating equipment: multi-layer coating machine, used to sequentially coat coatings containing fluorescent fibers arranged at different angles on the substrate. Others: agitator, oven, ultraviolet lamp, etc.
[0162] Steps and operations, Preparation of base fiber: Polyester chips are made into polyester fibers by melt spinning. Ensure that the fiber has good mechanical properties and processability. Weaving of triple parallel structure: Use a weaving machine to weave the polyester fiber into a triple parallel structure. Control the spacing between each row of fibers to ensure uniform coating of the subsequent fluorescent dye.
[0163] Treatment of fluorescent dyes: Dissolve red, green and blue fluorescent dyes in appropriate amounts of solvents. Use dipping or spraying methods to apply different colors of fluorescent dyes on the surface of each row of fibers. Ensure that the fluorescent dyes are evenly attached to the fiber surface and have a distinct fluorescent effect under ultraviolet light.
[0164] Surface modification of fiber: Prepare an aqueous solution containing hydroxy silane coupling agent. Immerse the triple parallel fluorescent fiber structure in the aqueous solution of the surface modifier. Control the temperature between 50°C and react for 3 hours. Ensure that the modifier is firmly grafted on the fiber surface to improve the bonding strength between the fiber and the coating and the fluorescent properties of the fiber.
[0165] Coating preparation and coating: Prepare water-based multi-fluorescent anti-counterfeiting coatings as needed to ensure that the coatings have good fluidity and film-forming properties. Arrange the surface-modified triple parallel fluorescent fiber structure at a preset angle K (such as 20°, 25°, 30°, etc.) and add it to the coating. Use multi-layer coating technology to sequentially coat the coating containing fluorescent fibers arranged at different angles on the substrate. Ensure that each layer of coating is evenly covered to form a coating with multiple fluorescent effects and complex anti-counterfeiting patterns.
[0166] Comparative Example 1
[0167] A water-based multiple fluorescent anti-counterfeiting coating and a preparation method thereof are provided, which is basically the same as that of Example 4, except that the polysiloxane-modified acrylic resin component in the water-based multiple fluorescent anti-counterfeiting coating is removed and is no longer used in the preparation step.
[0168] Comparative Example 2
[0169] A water-based multi-fluorescent anti-counterfeiting coating and a preparation method thereof are provided, which is basically the same as that of Example 4, except that the use of regenerated cellulose microfibers is omitted.
[0170] Comparative Example 3
[0171] A water-based multi-fluorescent anti-counterfeiting coating and a preparation method thereof are provided, which is basically the same as that of Example 4, except that quantum dots are removed and are not used in the preparation method.
[0172] Comparative Example 4
[0173] A water-based multi-fluorescent anti-counterfeiting coating and a preparation method thereof are provided, which is basically the same as that of Example 4, except that a cross-linking agent is omitted and the coating is not prepared using a cross-linking agent.
[0174] The water-based multi-fluorescent anti-counterfeiting coatings prepared in the above-mentioned Examples 1 to 4, Comparative Examples 1 to 2, and Comparative Examples 1 to 4 were tested;
[0175] Relevant testing standards:
[0176] GB / T 1728-1979 (1989) "Determination of drying time of paint films and putty films": Determine the drying time of paint to evaluate its curing speed and construction efficiency.
[0177] GB / T 1732-1993 "Determination of impact resistance of paint films": Tests the resistance of paint films when subjected to impact.
[0178] GB / T 9286-1998 "Scratch test for paint and varnish films": evaluates the adhesion of the paint film to the substrate.
[0179] GB / T 5210-2006 "Paint and varnish adhesion test by pull-off method": Determine the adhesion of the paint film by the pull-off method.
[0180] Customized fluorescence performance testing: Customized testing methods may be required for the special properties of fluorescent coatings, such as fluorescence intensity, fluorescence lifetime, fluorescence color, etc.
[0181] Detection method overview:
[0182] Drying time determination: Record the time required for the paint to completely dry after application.
[0183] Impact resistance determination: Use an impact testing machine to carry out impact test on the paint film.
[0184] Adhesion test: Evaluate the bonding strength between the paint film and the substrate by cross-cut test or pull-off method.
[0185] Fluorescence performance testing: Use fluorescence spectrometer and other equipment to measure indicators such as fluorescence intensity and fluorescence lifetime.
[0186] The results are shown in Table 1:
[0187] Table 1
[0188]
[0189] From the above Table 1, it can be clearly seen that the fluorescence intensity of Example 4 is the highest, which is 99 relative units, indicating that its fluorescence effect is most significant in the embodiment. Example 2 is slightly lower than Example 4, which is 98 relative units. The fluorescence intensity of Example 1 and Example 3 is the same, both of which are 97 relative units, slightly lower than the other two embodiments. Overall, the fluorescence intensity of the four embodiments is not much different, but Example 4 performs the best. Example 4 has the strongest impact resistance, which is 50kg·cm, showing good impact resistance. The impact resistance of Example 1 and Example 3 is the same, which is 49kg·cm, slightly lower than Example 4. The impact resistance of Example 2 is slightly lower, which is 48kg·cm, the lowest among the four embodiments. In terms of impact resistance, Example 4 also shows the best performance. The adhesion of all four embodiments is 5B, indicating that they perform consistently and well in adhesion performance. The drying time of the four embodiments is 4 hours, indicating that there is no difference in their drying speed. Based on the above analysis, the embodiments are basically consistent in terms of fluorescence intensity and impact resistance, and all embodiments are consistent in terms of adhesion and drying time. In various tests, embodiments 1 to 4 all perform well.
[0190] In control examples 1 and 2, the fluorescence intensity is 99 relative units compared to Example 4, which is lower than 120 relative units of Control Example 1 and 110 relative units of Control Example 2. This shows that in terms of fluorescence effect, Example 4 is not as significant as the two control examples. Control example 1 shows the highest fluorescence intensity because the linear arrangement of quantum dots optimizes the concentration and obviousness of the fluorescence effect; through the linear arrangement of quantum dots, the fluorescence intensity is enhanced because the arrangement makes the fluorescence effect of the quantum dots more concentrated and obvious.
[0191] In terms of impact resistance, both Example 4 and Comparative Example 1 are 50 kg·cm, showing the same impact resistance. However, Comparative Example 2 has a higher impact resistance of 55 kg·cm. The triple parallel fluorescent fiber structure increases the mechanical properties of the coating and the complexity of the fluorescent effect, which slightly improves the fluorescent intensity and enhances the hardness and impact resistance.
[0192] The adhesion of all the control examples and Example 4 is 5B, indicating that they are consistent and good in adhesion performance, with no significant difference. The drying time of Example 4 and Control Example 1 is 4 hours, while the drying time of Control Example 2 is 4.5 hours. This indicates that Control Example 2 may take a little longer to complete the drying process, which is related to the complexity of the triple parallel fluorescent fiber structure.
[0193] See attached Figure 1-2In Example 4 and Comparative Example 1 with the same other conditions, Comparative Example 1 reduces the use of polysiloxane-modified acrylic resin. After testing, the fluorescence intensity of Example 4 (99 relative units) of the finally prepared water-based multi-fluorescent anti-counterfeiting coating is significantly higher than that of Comparative Example 1 (80 relative units); the impact resistance of Example 4 (50kg·cm) is significantly better than that of Comparative Example 1 (30kg·cm); the adhesion of Example 4 (5B) is stronger than that of Comparative Example 1 (3B); the drying time of Example 4 (4 hours) is shorter than that of Comparative Example 1 (6 hours); after omitting the regenerated cellulose microfibers, the mechanical properties of the coating are reduced, but the fluorescence intensity remains basically unchanged.
[0194] In comparative example 2, the use of regenerated cellulose microfibers was omitted. After testing, the fluorescence intensity of Example 4 (99 relative units) was slightly higher than that of Comparative Example 2 (95 relative units). The difference is not big; the impact resistance of Example 4 (50kg·cm) is stronger than that of Comparative Example 2 (40kg·cm); the adhesion of Example 4 (5B) is better than that of Comparative Example 2 (4B); the drying time of the two is the same (4 hours), indicating that there is no significant difference in the drying speed between the two; after omitting the regenerated cellulose microfibers, the mechanical properties of the coating are reduced, but the fluorescence intensity remains basically unchanged;
[0195] In comparative example 3, quantum dots were removed and not used in the preparation. After testing, the fluorescence intensity of the water-based multi-fluorescent anti-counterfeiting coating finally prepared was much higher in Example 4 (99 relative units) than in comparative example 3 (50 relative units); the impact resistance of the two was the same (50 kg·cm), indicating that the two were equivalent in terms of resistance to external impact; the adhesion of the two was the same (5B), which means that there was no difference in the firmness of the bonding between the coating and the substrate; the drying time of the two was the same (4 hours), indicating that the two were consistent in terms of drying speed; after omitting the quantum dots, the fluorescence intensity was significantly reduced because the quantum dots were an important source of fluorescence in the coating;
[0196] In Comparative Example 4, the cross-linking agent was omitted, and after testing, the fluorescence intensity of Example 4 (99 relative units) of the finally prepared water-based multiple fluorescent anti-counterfeiting coating was significantly higher than that of Comparative Example 4 (90 relative units); the impact resistance of Example 4 (50kg·cm) was slightly stronger than that of Comparative Example 4 (45kg·cm); the adhesion of Example 4 (5B) was stronger than that of Comparative Example 4 (4B); the drying time of Example 4 (4 hours) was shorter than that of Comparative Example 4 (5 hours); after omitting the cross-linking agent, the stability and weather resistance of the coating were reduced, resulting in a decrease in both the fluorescence intensity and the physical properties.
[0197] In summary, the present invention is composed of multiple components, including polysiloxane-modified acrylic resin, regenerated cellulose microfibers, quantum dots, fluorescent fibers, etc., and the final product is obtained through a series of preparation steps. The linear arrangement of quantum dots is achieved by applying an external magnetic field to enhance the directionality and intensity of the fluorescent signal. The fluorescent fibers with a triple parallel structure are introduced to increase the visual complexity and anti-counterfeiting effect of the coating.
[0198] The fluorescent effect of the coating is significantly improved through the linear arrangement of quantum dots and the triple parallel fluorescent fiber structure. These special structures can enhance the directionality and intensity of the fluorescent signal, making the coating show brighter and clearer patterns under specific excitation light. The coating combines a variety of fluorescent materials and technologies, such as quantum dots and fluorescent fibers, which emit different colors of fluorescence under ultraviolet light excitation to form complex anti-counterfeiting patterns. This multiple fluorescent effect greatly improves the anti-counterfeiting performance of the coating; the coating adopts a water-based system, which reduces the use of harmful solvents and is more environmentally friendly. At the same time, the introduction of regenerated cellulose microfibers also reflects the utilization of renewable resources and enhances the environmental protection and sustainability of the coating. Due to the reinforcing effect of regenerated cellulose microfibers, the coating has excellent mechanical properties and can better resist erosion and damage from the external environment.
[0199] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A water-based multi-fluorescent anti-counterfeiting coating, characterized in that: The invention comprises the following components in parts by weight: 30-50 parts of polysiloxane-modified acrylic resin, 5-15 parts of regenerated cellulose microfibers, 1-10 parts of quantum dots, 1-5 parts of fluorescent fibers, 10-30 parts of water-based fluorescent pigments, 0.5-3 parts of crosslinking agents, 0.5-2 parts of dispersants and 20-60 parts of deionized water.
2. The water-based multi-fluorescent anti-counterfeiting coating according to claim 1, characterized in that: The invention comprises the following components in parts by weight: 40 parts of polysiloxane-modified acrylic resin, 7 parts of regenerated cellulose microfibers, 3 parts of quantum dots, 2 parts of fluorescent fibers, 20 parts of water-based fluorescent pigments, 2 parts of crosslinking agents, 1.5 parts of dispersants and 40 parts of deionized water.
3. A water-based multi-fluorescent anti-counterfeiting coating according to claim 1 or 2, characterized in that: The fluorescent fiber is a polymer material matrix, which includes polyester. Fluorescent substances are uniformly dispersed inside the fluorescent fiber. The fluorescent substances include fluorescent dyes and fluorescent pigments. The cross-linking agent uses a water-based blocked isocyanate curing agent. The dispersant is one of sodium polyacrylate and sodium dodecylbenzene sulfonate. The quantum dots are ZnS:Mn / ZnS core-shell structure quantum dots, the core is ZnS:Mn, the shell is pure ZnS, the particle size of the quantum dots is controlled between 5 and 10 nanometers, the fluorescence emission wavelength of the quantum dots is concentrated between 520 and 530 nanometers, and the half-peak width is less than 30 nanometers. The water-based fluorescent pigment is a rhodamine B-based fluorescent pigment, and the particle size is controlled between 1 and 5 microns.
4. A water-based multi-fluorescent anti-counterfeiting coating according to claim 1 or 2, characterized in that: The polysiloxane-modified acrylic resin is a composite of an acrylic resin with a glycidyl group and a siloxane prepolymer with a number average molecular weight of 1000-2000 through copolymerization or grafting, wherein the weight ratio of the acrylic resin to the siloxane prepolymer is 20:80; the diameter of the regenerated cellulose microfiber is 0.5-0.8 microns, the length is 50-100, the ellipticity of the regenerated cellulose microfiber is less than 1.5, and the surface of the regenerated cellulose microfiber is carboxylated, and the carboxyl content reaches 2% of the total weight of the fiber.
5. The water-based multi-fluorescent anti-counterfeiting coating according to claim 1, characterized in that: The polysiloxane-modified acrylic resin contains active groups, including hydroxyl groups and carboxyl groups; The surface of the regenerated cellulose microfiber is treated with a surface modifier A, and the surface modifier A forms a hydrogen bond or a covalent bond with the polysiloxane-modified acrylic resin; The surface of the quantum dots is coated with a layer of organic ligands, the organic ligands contain carboxyl groups or amino groups, the organic ligands are compatible with the polysiloxane-modified acrylic resin, and the linear arrangement of the quantum dots is achieved through the guidance of an external magnetic field or electric field; The fluorescent fiber has a triple parallel fluorescent fiber structure. The surface of each row of fibers is treated with different fluorescent dyes. The triple parallel fluorescent fiber structure is arranged at an angle in the coating. The angle between the nth row of fluorescent fibers and the baseline is set to \theta_n, then: \theta_n=\theta_0+(n-1)\times\Delta\theta; Wherein, \theta_0 is the reference angle of the first row of fluorescent fibers; n is the number of rows of fluorescent fibers, counting from 1; \Delta\theta is the angle increment between two adjacent rows of fluorescent fibers; The surface of the pigment particles of the water-based fluorescent pigment is treated with a surface modifier B, and the surface modifier B forms a strong interaction with the polysiloxane-modified acrylic resin; The crosslinking agent is a crosslinking agent with a bifunctional group, one end of which reacts with the polysiloxane-modified acrylic resin, and the other end of which reacts with the surface modifier A to form a three-dimensional network structure.
6. A method for preparing a water-based multi-fluorescent anti-counterfeiting coating, characterized in that: The following steps are involved: S1: Selecting an acrylic resin with a glycidyl group as the main body, mixing the acrylic resin with a siloxane prepolymer with a number average molecular weight of 1000 to 2000 in a weight ratio of 20:80, and compounding by copolymerization or grafting at a temperature of 70 to 90° C. for 2 to 4 hours to form a polysiloxane-modified acrylic resin; S2: performing surface coating treatment on the quantum dots, selecting an organic ligand containing a carboxyl group or an amino group as the coating layer, and firmly connecting the ligand to the surface of the quantum dots through chemical bonding at a temperature of 50 to 70° C., and the reaction time is 1 to 3 hours; S3: performing surface modification treatment on the fluorescent fiber, selecting a silane coupling agent containing a hydroxyl group, an amino group or an epoxy group as the surface modifier A, and firmly grafting the modifier on the fiber surface through a chemical reaction at a temperature of 40 to 60° C., and the reaction time is 2 to 4 hours; S4: performing surface modification treatment on pigment particles of water-based fluorescent pigment, selecting polyethylene glycol-grafted carboxylic acid as surface modifier B, and firmly adsorbing the modifier on the surface of pigment particles by physical adsorption or chemical bonding at a temperature of 30 to 50° C., and the reaction time is 1 to 2 hours; S5: taking the polysiloxane-modified acrylic resin as the main resin, adding an appropriate amount of deionized water for dilution to form a resin aqueous solution with a solid content of 30% to 50%; S6: adding fluorescent particles consisting of surface-modified quantum dots, fluorescent fibers and water-based fluorescent pigments to the resin aqueous solution, and uniformly dispersing the fluorescent particles in the polysiloxane-modified acrylic resin by an ultrasonic dispersion method, wherein the ultrasonic frequency is 20 to 40 kHz and the dispersion time is 30 to 60 minutes to obtain a composite resin solution; S7: adding a dispersant to the composite resin solution to further ensure the dispersibility and stability of the composite resin solution environment; S8: A cross-linking agent with a bifunctional group is selected and added, one end of which reacts with the active group in the polysiloxane-modified acrylic resin, and the other end reacts with the modifier on the surface of the fluorescent particles to form a three-dimensional network structure, so that the coating forms a stable cross-linked network structure to obtain a water-based multi-fluorescent anti-counterfeiting coating.
7. The method for preparing a water-based multi-fluorescent anti-counterfeiting coating according to claim 6, characterized in that: In S2, the linear arrangement of the quantum dots is achieved by applying an external magnetic field, the quantum dots are dispersed in a solvent to form a stable solution, an electromagnet or a permanent magnet is used to generate the required magnetic field, and the direction and intensity of the magnetic field are adjusted, and the quantum dot solution is placed in the magnetic field. Under the action of the magnetic force, the quantum dots are gradually arranged along the direction of the magnetic field to achieve linear arrangement. The relationship between the magnetic moment of the quantum dots and the magnetic field gradient is: F_m=\mu_0\cdotm\cdot\nablaB; Among them, F_m is the magnetic force on the quantum dot, \mu_0 is the magnetic permeability of the vacuum, m is the magnetic moment of the quantum dot, and \nablaB is the magnetic field gradient; Calculation of quantum dot magnetic moment: m=n\cdot\mu_B\cdotg_J\cdotJ; Where n is the number of magnetic ions in the quantum dot, \mu_B is the Bohr magneton, g_J is the Lande g factor, and J is the total angular momentum of the quantum dot; Calculation of magnetic field gradient: \nablaB=\frac{B_2-B_1}{d}; Among them, B_2 and B_1 are the magnetic field intensities at two different positions in the direction of quantum dot arrangement, and d is the distance between the two positions.
8. The method for preparing a water-based multi-fluorescent anti-counterfeiting coating according to claim 6, characterized in that: In S3, the fluorescent fiber comprises a base fiber material, and the base fiber material comprises polyester fiber; The basic fibers are woven into a triple parallel structure using textile technology, with spacing between each row of fibers. The surface of each row is treated with fluorescent dyes of different colors. A silane coupling agent containing a hydroxyl group, an amino group or an epoxy group is selected as a surface modifier. The triple parallel fluorescent fiber structure is immersed in an aqueous solution of the surface modifier, and the temperature is controlled between 40 and 60° C. The reaction is performed for 2 to 4 hours to firmly graft the modifier on the fiber surface. The triple parallel fluorescent fiber structure after surface modification is arranged at a preset angle K and added to the coating. Using multi-layer coating technology, coatings containing fluorescent fibers arranged at different angles are applied to the substrate in sequence to form a coating with multiple fluorescent effects and complex anti-counterfeiting patterns.
9. The method for preparing a water-based multi-fluorescent anti-counterfeiting coating according to claim 6, characterized in that: The S4 further includes S41: using a high-speed disperser to disperse the regenerated cellulose microfibers in deionized water, with the dispersion speed controlled at 8000-12000 rpm and the dispersion time at 10-30 minutes to form a uniform fiber suspension, and during the dispersion process, controlling the temperature of the suspension to be between 20° C. and 30° C.
10. The method for preparing a water-based multi-fluorescent anti-counterfeiting coating according to claim 6, characterized in that: In the S8, at a temperature of 50 to 70° C., a cross-linking agent with a bifunctional group is selected and added, one end of the cross-linking agent reacts with the active group in the polysiloxane-modified acrylic resin, and the other end reacts with the modifier on the surface of the fluorescent particles to form a three-dimensional network structure. The cross-linking and curing reaction time is 2 to 6 hours, so that the coating forms a stable cross-linked network structure to obtain a water-based multiple fluorescent anti-counterfeiting coating.
Citation Information
Patent Citations
Triple anti-forge material and triple anti-forge paper product thereof
CN100999881A
Nano fluorescence fiber
CN101177799A
Method for preparing nano colouring matter aqueous dispersions
CN101362865A
Material for preparation of fluorescent anti-counterfeiting mark
CN104693653A
Anti-doodling fluorescent water paint for interior wall and preparation method of water paint