Boron-doped silicon negative electrode material and preparation method thereof
By preparing B-doped Si negative electrode materials in lithium-ion batteries, the problems of volume expansion and insufficient conductivity of silicon materials during the charge and discharge process are solved, and the Coulombic efficiency and cycle stability of the first cycle are improved, which is suitable for high-specific energy lithium batteries. of industrial production.
Patent Information
- Application Number
- CN202410080293.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-19
- Publication Date
- 2024-10-29
AI Technical Summary
The low theoretical specific capacity of traditional graphite anode materials in lithium-ion batteries, the volume expansion of silicon anode materials during charge and discharge, and low intrinsic conductivity limit their commercial development, and existing boron-doped silicon materials have a Coulombic The efficiency improvement effect is not significant.
By mixing silicon and LiBH4 in a certain proportion under air-isolated conditions, performing high-energy ball milling, and heating to 400°C in an inert gas atmosphere to maintain the temperature, a B-doped Si anode material is prepared, which improves the diffusion rate of lithium ions and the circulation of the material. stability.
The first-cycle Coulombic efficiency of the silicon-based negative electrode material for lithium-ion batteries has been achieved above 99%, and has good cycle stability. At the same time, the process is simple and low-cost, making it suitable for large-scale industrial production.
Smart Images

Figure CN118867149A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of preparation of lithium ion battery negative electrode materials, and in particular relates to a boron-doped silicon negative electrode material and a preparation method thereof. Background Art
[0002] Lithium-ion batteries are one of the most widely used secondary batteries due to their high specific capacity, excellent cycle performance, and environmental friendliness. Currently, the application of lithium-ion batteries has expanded from portable devices such as mobile phones and laptops to electric vehicles and energy storage power stations. However, the low theoretical specific capacity of traditional graphite anodes makes it difficult to meet the demand for high-energy-density batteries. Therefore, developing a high-energy-density anode to replace graphite has become a research hotspot for lithium battery anode materials.
[0003] Silicon, with its extremely high specific capacity, low discharge voltage, and abundant reserves, is considered one of the most promising alternatives. However, silicon anode materials experience significant volume expansion during charge and discharge, leading to cracking and differentiation of the electrode material, and gradually losing contact with the current collector and conductive network. Furthermore, their low intrinsic conductivity leads to poor rate performance, limiting their commercial development.
[0004] To address the above problems, the most common method currently is to use conductive materials and nano-silicon powder for compounding or coating to alleviate the volume expansion of silicon and improve conductivity. Boron-doped silicon forms a P-type semiconductor. The more impurities incorporated, the higher the hole concentration, the better the conductivity and lithium ion diffusion, leading to improved material rate performance. At the same time, boron has a high elastic modulus and hardness, which effectively inhibits the huge volume expansion of silicon, improving cycle life and stability. For example, patent CN113809310A proposes a boron-doped soft carbon-coated silicon-based lithium ion negative electrode material and its preparation method. Using high-boiling-point boron-containing compounds and boron gas sources as doping materials, a boron-doped silicon-based negative electrode material is prepared by chemical vapor deposition, achieving high cycle stability, but the first-cycle coulomb efficiency is not significantly improved. Patent CN113130878B proposes using crystalline silicon cutting waste to obtain a boron-doped silicon-based negative electrode through pickling, centrifugation, washing, ultrasonic activation, and drying. The material obtained by this method has generally improved cycle stability. Therefore, it is necessary to develop a silicon-based negative electrode material and a preparation method thereof that has good electrochemical performance, low cost, simple process, and can be produced industrially on a large scale. Summary of the Invention
[0005] The present invention provides a boron-doped silicon anode material and a preparation method thereof, which can increase the first-cycle coulombic efficiency of the silicon-based anode material for lithium-ion batteries to above 99%, while having good cycle stability, simple process, and economical and efficient production.
[0006] A method for preparing a boron-doped silicon negative electrode material comprises the following steps: (1) Si and LiBH4 are mixed in a certain ratio in an airtight environment (H2O < 0.01 ppm, O2 < 0.01 ppm) to obtain a mixture; (2) subjecting the mixture to high-energy ball milling under an inert gas atmosphere; (3) The product is placed in a vacuum and heated to a predetermined temperature and kept warm to obtain a B-doped Si negative electrode material.
[0007] In the above steps, the molar ratio of Si to LiBH4 in step (1) is 1-9; The inert gas in step (2) is argon, helium or nitrogen; the high-energy ball mill is a planetary ball mill with a ball-to-material ratio of 160:1, a ball mill revolution speed of 400 rpm, and a ball milling time of 5 hours; high-energy ball milling of Si and LiBH4 is fast and efficient, can achieve material refinement and uniform mixing, and is more conducive to subsequent reactions; the setting of the high-energy ball milling ball-to-material ratio directly affects the ball milling effect. If the ball-to-material ratio is too low, it may lead to poor ball milling effect; if the ball-to-material ratio is too high, the energy consumption is large. A reasonable ball-to-material ratio can give full play to the impact and friction of the ball. Step (3) The product obtained after ball milling is transferred to a stainless steel reaction tube, dynamically vacuumed, heated to 400°C at a heating rate of 5°C / min and kept warm for 4 hours to allow LiBH4 to fully react, and then cooled to room temperature to obtain B-doped Si negative electrode material; an appropriate temperature should be selected. If the temperature is too low, LiBH4 cannot react completely; if the temperature is too high, the product will not form.
[0008] Beneficial effects: The present invention provides a boron-doped silicon negative electrode material and a preparation method thereof. The oxide layer on the Si surface affects the diffusion of lithium ions and reduces the electrochemical reaction kinetics. At the same time, the oxide layer on the Si surface will break during the cycle, forming a large amount of irreversible products, resulting in a low first coulombic efficiency. The present invention improves the diffusion rate of lithium ions by B doping, and the reducing gas atmosphere generated during the thermal decomposition process of LiBH4 reduces the Si surface oxide layer, significantly improving the first-cycle coulombic efficiency, and increasing the first-cycle coulombic efficiency of the silicon-based negative electrode material for lithium-ion batteries to more than 99%; at the same time, it also has good cycle stability; and the preparation process of the present invention is simple, has low equipment requirements, low cost, and high economic benefits, and can be applied to the large-scale production of high-energy-density lithium batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 This is the X-ray diffraction pattern of the boron-doped silicon negative electrode material obtained in Examples 1-5 of the present invention; Figure 2 This is the X-ray diffraction pattern of the boron-doped silicon negative electrode material obtained in Example 5 of the present invention; Figure 3 This is a graph showing the first charge and discharge efficiency of the boron-doped silicon negative electrode material obtained in Examples 1-5 of the present invention; Figure 4 This is a first cycle charge and discharge curve of the boron-doped silicon negative electrode material obtained in Example 5 of the present invention; Figure 5 This is a long cycle diagram of the boron-doped silicon negative electrode material obtained in Example 5 of the present invention. DETAILED DESCRIPTION
[0010] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments: Example 1
[0011] A method for preparing a boron-doped silicon negative electrode material comprises the following steps: in an air-tight state (H2O <0.01 ppm, O2 <0.01 ppm), firstly mixing Si and LiBH4 at a molar ratio of 9:1 in a mortar and uniformly transferring the mixture to a stainless steel ball milling jar, then using a planetary ball mill for high-energy ball milling, and sealing the mixture for ball milling in a high-purity (99.999%) argon atmosphere at a ball milling speed of 400 rpm for 5 hours, wherein the ball-to-material ratio is 160:1; and after ball milling, transferring the product to a stainless steel reaction tube for dynamic vacuum heating at a heating rate of 5°C / min to 400°C, holding the mixture for 4 hours, and cooling the mixture to room temperature to obtain a B-doped Si negative electrode material. Example 2
[0012] A method for preparing a boron-doped silicon negative electrode material comprises the following steps: in an air-tight state (H2O <0.01 ppm, O2 <0.01 ppm), firstly mixing Si and LiBH4 in a molar ratio of 8:2 in a mortar and uniformly transferring the mixture to a stainless steel ball mill jar, then using a planetary ball mill for high-energy milling, sealing and ball milling in a high-purity (99.999%) argon atmosphere, at a ball milling speed of 400 rpm, for 5 hours, wherein the ball-to-material ratio is 160:1; and transferring the product to a stainless steel reaction tube, performing dynamic vacuum heating at a heating rate of 5°C / min to 400°C, holding the mixture for 4 hours, and cooling the mixture to room temperature to obtain a B-doped Si negative electrode material. Example 3
[0013] A method for preparing a boron-doped silicon negative electrode material comprises the following steps: in an air-tight state (H2O <0.01 ppm, O2 <0.01 ppm), firstly mixing Si and LiBH4 in a molar ratio of 7:3 using a mortar and uniformly transferring the mixture to a stainless steel ball mill jar, then using a planetary ball mill for high-energy ball milling, sealing the mixture in a high-purity (99.999%) argon atmosphere at a ball milling speed of 400 rpm for 5 hours, wherein the ball-to-material ratio is 160:1; and transferring the product to a stainless steel reaction tube for dynamic vacuum heating at a heating rate of 5°C / min to 400°C, holding the mixture for 4 hours, and cooling the mixture to room temperature to obtain a B-doped Si negative electrode material. Example 4
[0014] A method for preparing a boron-doped silicon negative electrode material comprises the following steps: in an air-tight state (H2O <0.01 ppm, O2 <0.01 ppm), first mixing Si and LiBH4 in a molar ratio of 6:4 using a mortar and uniformly transferring the mixture to a stainless steel ball mill jar, then using a planetary ball mill for high-energy ball milling, sealed ball milling in a high-purity (99.999%) argon atmosphere, with a ball mill revolution speed of 400 rpm and a ball milling time of 5 hours, wherein the ball-to-material ratio is 160:1; transferring the product to a stainless steel reaction tube, performing dynamic vacuum heating at a heating rate of 5°C / min to 400°C, holding the mixture at this temperature for 4 hours, and cooling the mixture to room temperature to obtain a B-doped Si negative electrode material. Example 5
[0015] A method for preparing a boron-doped silicon negative electrode material comprises the following steps: in an air-tight state (H2O <0.01 ppm, O2 <0.01 ppm), first mixing Si and LiBH4 at a molar ratio of 1:1 in a mortar and uniformly transferring the mixture to a stainless steel ball mill jar, then using a planetary ball mill for high-energy milling, sealing the mixture in a high-purity (99.999%) argon atmosphere at a milling speed of 400 rpm for 5 hours, wherein the ball-to-material ratio is 160:1; transferring the product to a stainless steel reaction tube, performing dynamic vacuum heating at a heating rate of 5°C / min to 400°C, holding the mixture for 4 hours, and cooling the mixture to room temperature to obtain a B-doped Si negative electrode material.
[0016] Figure 1 This is the X-ray diffraction pattern of the boron-doped silicon negative electrode material obtained in Example 1-5. It can be found that LiBH4 is completely decomposed during the heating process.
[0017] Figure 2 This is the X-ray diffraction pattern of the boron-doped silicon negative electrode material obtained in Example 5. It can be found that a B-Si amorphous nanolayer is formed on the surface of Si.
[0018] Figure 3 The first charge and discharge efficiency diagram of the boron-doped silicon negative electrode material obtained in Examples 1 to 5 is shown. Figure 2 From the comparison, it can be found that the first-cycle Coulombic efficiency of the sample obtained in Example 5 is as high as 99.55%, which is the best effect. High first-cycle Coulombic efficiency means stable SEI formation and reduced side reactions.
[0019] Figure 4 This is the first cycle charge-discharge curve of the boron-doped silicon negative electrode material obtained in Example 5. By comparing the first cycle charge-discharge curve of pure Si, it can be seen that boron doping plays an important role and the first cycle coulombic efficiency is significantly improved.
[0020] Figure 5 This is a long cycle diagram of the boron-doped silicon negative electrode material obtained in Example 5. It can be seen that the boron-doped sample has good cycle stability.
[0021] The above-described embodiments are only preferred embodiments of the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or modifications made by those skilled in the art based on the present invention are all within the protection scope of the present invention.
Claims
1. A method for preparing a boron-doped silicon negative electrode material, characterized in that: The following steps are involved: Si and LiBH4 are mixed in an air-tight condition to obtain a mixture; The mixture was subjected to high-energy ball milling under an inert gas atmosphere; The ball-milled mixture is placed in a vacuum, heated to a predetermined temperature, and kept warm to obtain a B-doped Si negative electrode material.
2. The method for preparing a boron-doped silicon negative electrode material according to claim 1, characterized in that: The molar ratio of Si to LiBH4 is 1-9.
3. The method for preparing a boron-doped silicon negative electrode material according to claim 1 or 2, characterized in that: The air isolation conditions are H2O<0.01 ppm, O2<0.01 ppm.
4. The method for preparing a boron-doped silicon negative electrode material according to claim 1, characterized in that: The inert gas is argon, helium or nitrogen.
5. The method for preparing a boron-doped silicon negative electrode material according to claim 1, characterized in that: The high energy ball mill is a planetary ball mill.
6. The method for preparing a boron-doped silicon negative electrode material according to claim 1 or 5, characterized in that: The ball-to-material ratio of the high-energy ball mill is 160:1, the ball mill revolution speed is 400 revolutions per minute, and the ball mill time is 5 hours.
7. The method for preparing a boron-doped silicon negative electrode material according to claim 1, characterized in that: Heating in a vacuum is dynamic vacuuming.
8. The method for preparing a boron-doped silicon negative electrode material according to claim 1, characterized in that: The heating rate was 5°C / min, the heating temperature was 400°C, and the holding time was 4 hours.
9. The boron-doped silicon negative electrode material prepared by the method according to any one of claims 1 to 8, characterized in that: The silicon negative electrode material reduces the Si surface oxide layer by reducing gas generated by B doping and LiBH4 thermal decomposition, and a B-Si amorphous nanolayer is formed on the surface of Si.
Citation Information
Patent Citations
Transition-metal fluoride loaded boron-doped nano-carbon composite material preparation method
CN106910891A
Boron-doped silicon-based negative electrode material used for lithium ion battery
CN107195893A
Method for preparing boron-doped porous carbon spheres
CN107346821A
Soft carbon-coated boron-doped silicon-based negative electrode material and preparation method and application thereof
CN113363430A
Carbon-coated hollow silicon material and preparation method and application thereof
CN113636561A