Silicon nitride sintered body

By adding yttrium silicon oxynitride particles to the silicon nitride sintered body and controlling the porosity, the problem of reduced thermal conductivity and insufficient mechanical properties in high temperature environments is solved, achieving efficient heat dissipation and improved stability, and is suitable for high temperature power modules .

CN118871407APending Publication Date: 2024-10-29KYOCERA CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380023526.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-25
Filing Date
2023-02-13
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The thermal conductivity of existing silicon nitride sintered bodies decreases in high-temperature environments, making it difficult to stably maintain efficient heat dissipation. Moreover, the mechanical properties are insufficient during temperature cycles, which affects the stability of the power module.

Method used

A silicon nitride sintered body containing silicon nitride particles and yttrium silicon oxynitride particles is used. The porosity is controlled below 14%. Through a specific composition ratio and heat treatment process, its thermal conductivity and fracture toughness at high temperatures are improved.

Benefits of technology

It maintains high thermal conductivity and heat dissipation in high-temperature environments, and improves fracture toughness and insulation voltage resistance. It is suitable for use in high-temperature power modules, ensuring stable driving of power components and stable operation of power modules.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005008267430000041
    Figure BDA0005008267430000041
  • Figure BDA0005008267430000051
    Figure BDA0005008267430000051
  • Figure BDA0005008267430000052
    Figure BDA0005008267430000052
Patent Text Reader

Abstract

The silicon nitride-based sintered body according to the present invention contains silicon nitride particles and yttrium silicon oxynitride (Yttrium Silicon Oxynitride) particles, and has a porosity of 14% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a silicon nitride sintered body. Background Art

[0002] Conventionally, silicon nitride sintered bodies have attracted attention as materials excellent in heat resistance, strength, and hardness, and have been used, for example, as engine parts.

[0003] In recent years, power modules that convert and control electric power with high efficiency have been used in electric vehicles and the like. Power modules require not only insulation properties but also an insulating substrate having high thermal conductivity for efficiently transferring heat generated from semiconductor elements and high mechanical properties capable of withstanding stress caused by temperature cycles. As a material for an insulating substrate that meets such requirements, the present applicant has previously disclosed a silicon nitride sintered body as shown in the following Patent Document 1.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent document 1: International Publication No. 2005 / 019133. Summary of the invention

[0007] A silicon nitride sintered body according to one embodiment of the present invention contains silicon nitride particles and yttrium silicon oxynitride particles, and has a porosity of 14% or less. DETAILED DESCRIPTION

[0008] Hereinafter, a mode for implementing the silicon nitride sintered body of the present invention (hereinafter referred to as “embodiment”) will be described in detail with reference to the drawings.

[0009] In recent years, for example, power modules used in electric vehicles have tended to operate at higher temperatures for the purpose of high efficiency and energy saving. Therefore, there is a demand for silicon nitride sintered bodies that can be used stably even in higher temperature environments.

[0010] The silicon nitride sintered body of the embodiment contains silicon nitride particles and yttrium silicon oxynitride particles, and the porosity is less than 14%. The above silicon nitride sintered body is more suitable for use in a high temperature environment. Specifically, the silicon nitride sintered body of the embodiment can maintain a high thermal conductivity even in a high temperature environment (e.g., about 100 to 200°C). That is, the silicon nitride sintered body according to the embodiment is suitable for use in a high temperature environment because it can maintain high thermal conductivity and heat dissipation in a high temperature environment.

[0011] The silicon nitride sintered body of the embodiment may contain Y6Si 11 N 20At least one of YSi3O3N4 particles (hereinafter referred to as "phase A"), Y4Si2O7N2 particles (hereinafter referred to as "phase C") and Y2Si3O3N4 particles (hereinafter referred to as "phase D") is used as yttrium silicon oxynitride particles.

[0012] In addition, the silicon nitride sintered body of the embodiment may contain two of the phase A, phase B, phase C, and phase D as yttrium silicon oxynitride particles. Specifically, the silicon nitride sintered body of the embodiment may contain both the phase A and the phase B. In addition, the silicon nitride sintered body of the embodiment may contain both the phase C and the phase D.

[0013] In the silicon nitride sintered body of the embodiment, the volume ratio of phase A / phase B (ratio of phase A to phase B) may be 1.4 or more. By setting the above configuration, a silicon nitride sintered body having a thermal conductivity of 67 W / m·K or more at 100°C and a thermal conductivity of 49 W / m·K or more at 200°C can be obtained.

[0014] In the silicon nitride sintered body of the embodiment, the volume ratio of phase A / phase B (ratio of phase A to phase B) may be 2.0 or more. By setting the above configuration, a silicon nitride sintered body having a thermal conductivity of 72 W / m·K or more at 100°C and a thermal conductivity of 55 W / m·K or more at 200°C can be obtained.

[0015] In the silicon nitride sintered body of the embodiment, the volume ratio of phase A / phase B (ratio of phase A to phase B) may be 3.0 or more. By setting the above configuration, a silicon nitride sintered body having a thermal conductivity of 74 W / m·K or more at 100° C. and a thermal conductivity of 57 W / m·K or more at 200° C. can be obtained.

[0016] The fracture toughness of the silicon nitride sintered body of the embodiment can be 6.5 MPa·m 1 / 2 As described above, the dielectric withstand voltage can be 10 kV or more, and the three-point bending strength can be 521 MPa or more. According to the above configuration, a silicon nitride sintered body having excellent magnetic properties can be obtained.

[0017] (Example)

[0018] Si3N4 powder, Si powder, Y2O3, and MgO are mixed at a ratio of 23.4wt%, 70.2wt%, 4.9wt%, and 1.5wt% to obtain a raw powder. Y2O3 and MgO are sintering aids. Then, the raw powder, ethanol, and silicon nitride crushing media are put into a drum mill for mixing. Then, polyvinyl alcohol (PVA) is added to the obtained slurry as an organic binder and mixed, and then granulated using a spray dryer. The obtained granulated powder is molded under a molding pressure of 80MPa by a powder pressing molding method using a mold, and degreased at 600°C in N2 to obtain a plurality of molded bodies.

[0019] Then, the obtained molded body was heat treated under the conditions of nitrogen partial pressure (0.3 MPa or 0.6 MPa), temperature (1350°C), and time (15 hours) shown in Table 1, thereby performing a nitriding step of nitriding Si in the molded body to Si3N4. Then, the temperature was further raised, and the molded body was fired under the conditions of temperature (1900°C, 1925°C, or 1945°C) and time (6 hours or 12 hours) shown in Table 1 at the same nitrogen partial pressure as in the nitriding step, thereby obtaining the samples (No. 1 to No. 5) of the present invention.

[0020] In addition, Si3N4 powder, Si powder, Y2O3, and MgO are mixed in a ratio of 65.5wt%, 21.9wt%, 11.9wt%, and 0.7wt% to obtain a raw powder. Y2O3 and MgO are sintering aids. Then, the raw powder, ethanol, and silicon nitride pulverizing media are put into a drum mill for mixing. Then, polyvinyl alcohol (PVA) is added to the obtained slurry as an organic binder and mixed, and then granulated using a spray dryer. The obtained granulated powder is molded under a molding pressure of 80MPa by a powder pressing molding method using a mold, and degreased at 600°C in N2 to obtain a plurality of molded bodies.

[0021] Then, the obtained molded body was subjected to nitriding treatment under normal pressure and the conditions shown in Table 1. In addition, for sample No. 8, a nitriding process was performed to nitride Si in the molded body to Si3N4 by heat treatment at 1100°C to 1400°C for 40 hours. Then, it was sintered at 0.7MPa, 1900°C, and 12 hours to obtain the sample of the present invention (No. 8). It should be noted that "1100°C to 1400°C" means that the heat treatment is performed while raising the temperature from 1100°C to 1400°C for 40 hours.

[0022] In Table 1, sample numbers 6 and 7 are shown as comparative examples. Sample number 6 is a silicon nitride sintered body described in Japanese Patent Gazette No. 6822362. The manufacturing method of sample number 6 is as follows. Si powder, Y2O3, and MgO are mixed at a ratio of 89.0wt%, 1.2wt%, and 9.8wt% to obtain a raw material powder. To the raw material powder, a dispersant (sorbitan trioleate) is added in an amount of 0.5wt% relative to the total of the dispersion medium (toluene) and the raw material powder to form a slurry with a concentration of 42wt%, and the slurry is crushed for 24 hours using a ball mill using 5φ balls made of silicon nitride as the medium.

[0023] To the obtained slurry, a dispersion medium and an organic binder (acrylic resin) are added to adjust the concentration, and a degassing treatment is performed to prepare a slurry-like coating liquid. The coating slurry is formed into a sheet by a scraper method to obtain a sheet-like molded body. After degreasing the obtained sheet-like molded body, it is nitrided for 10 hours in a boron nitride (Boron Nitride, BN) crucible under a nitrogen environment (nitrogen partial pressure 0.1MPa) and 1450°C, and then sintered for 12 hours in a boron nitride (BN) crucible under a nitrogen environment (nitrogen partial pressure 0.9MPa) and 1900°C to obtain sample No. 6.

[0024] In addition, sample number 7 is a silicon nitride sintered body described in Japanese Patent Gazette No. 6297188. The manufacturing method of sample number 7 is as follows. Si3N4 powder, Y2O3, and MgO are mixed at a ratio of 95.0wt%, 3wt%, and 2wt% to obtain a raw material powder. A dispersion medium and an organic solvent are mixed in the raw material powder and mixed in a ball mill. Then, with respect to 100 parts by mass of the raw material powder, 10 parts by mass of butyl methacrylate as an organic binder and 4 parts by mass of dibutyl phthalate as a plasticizer are mixed, and the organic solvent is added, and the ball mill is fully mixed to prepare a slurry-like raw material mixture. After adjusting the viscosity of the slurry to 5000-15000cps, the sheet is formed and dried by a sheet forming method (scraper method) to prepare a molded body (green sheet). In a nitrogen environment, the molded body is heated at 500-800°C for 1-4 hours to perform a degreasing process. Then, the degreased compact was sintered at 1900° C. for 9 hours in a nitrogen atmosphere, thereby obtaining Sample No. 7.

[0025] [Table 1]

[0026]

[0027] The components of Si3N4 powder, Si powder, Y2O3, and MgO used as raw materials for sample No. 1 to No. 5 and No. 8 of the embodiment were analyzed. The results are shown in Tables 2 to 4. The Si3N4 powder was subjected to X-ray Fluorescence (XRF) analysis and Inductively Coupled Plasma (ICP) emission spectrometry analysis (Table 2). In addition, the Si powder, Y2O3, and MgO were subjected to X-ray Fluorescence (XRF) analysis (Tables 3 and 4).

[0028] [Table 2] [Table 3]

[0029] [Table 4]

[0030] It is known that Si3N4 powder, Si powder, Y2O3, and MgO used as raw materials contain the impurities shown in Tables 2 to 4. Specifically, Si3N4 powder contains Al2O3, CaO, and Fe2O3 in addition to Si3N4, Si powder contains O, Fe, Ni, and K in addition to Si, Y2O3 contains SiO2, Fe2O3, Cr2O3, and CaF2, and MgO contains SiO2, Al2O3, CaO, Fe2O3, and B2O3.

[0031] The samples No. 1 to No. 5 of the examples were pulverized, and the crystal phases were identified by X-ray diffraction, and then the ratio of each crystal phase was determined by the Rietveld method. The results are shown in Table 5.

[0032] [Table 5]

[0033]

[0034] As shown in Table 5, Sample Nos. 1 to 5 and 8 all contain silicon nitride particles and yttrium silicon oxynitride particles. Specifically, Sample Nos. 1 to 5 contain β-phase SiN as silicon nitride particles. In addition, Sample Nos. 1 to 5 contain Y6Si 11 N 20 O particles (phase A) and YSi3O3N4 particles (phase B) as yttrium silicon oxynitride particles. In addition, sample number 8 contains β-phase SiN as silicon nitride particles. In addition, sample number 8 contains Y4Si2O7N2 particles (phase C) and Y2Si3O3N4 particles (phase D) as yttrium silicon oxynitride particles.

[0035] Regarding the volume ratio of phase A to phase B (phase A / phase B), sample number 1 is "2.0", sample number 2 is "3.1", sample number 3 is "1.4", sample number 4 is "0.1", and sample number 5 is "0.2".

[0036] (Porosity)

[0037] For Sample Nos. 1 to 5 and 8, each sample was polished, and the polished surface was photographed using an electron microscope to extract the pores present in the unit area (20 μm×20 μm) of the obtained photograph. Then, the area of ​​the extracted pores was calculated by image analysis, and the area ratio based on the unit area was calculated.

[0038] As shown in Table 5, the porosity of Sample No. 1 to No. 5 and No. 8 is "0.5%" for Sample No. 1, "0.9%" for Sample No. 2, "0.4%" for Sample No. 3, "13.6%" for Sample No. 4, "11.3%" for Sample No. 5, and "0.3%" for Sample No. 8. In addition, the porosity of Sample No. 6 as a comparative example is "1.5%".

[0039] For Sample Nos. 1 to 5 and 8, a 10 mm square, 0.32 mm thick test piece was cut out from each sample, and the thermal conductivity in the thickness direction of the cut test piece was measured using the laser flash method. The measurement temperatures were room temperature, 100°C, and 200°C. The results are shown in Table 6.

[0040] [Table 6]

[0041]

[0042] As shown in Table 6, regarding the thermal conductivity at room temperature, sample No. 1 is "94 W / m·K", sample No. 2 is "96 W / m·K", sample No. 3 is "86 W / m·K", sample No. 4 is "76 W / m·K", sample No. 5 is "81 W / m·K", and sample No. 8 is "88 W / m·K". In addition, the thermal conductivity of sample Nos. 6 and 7 as comparative examples is "123 W / m·K" and "90 W / m·K", respectively.

[0043] In addition, regarding the thermal conductivity under the condition of 100°C, sample number 1 is "72 W / m·K", sample number 2 is "74 W / m·K", sample number 3 is "67 W / m·K", sample number 4 is "57 W / m·K", sample number 5 is "61 W / m·K", and sample number 8 is "62 W / m·K". In addition, the thermal conductivity of sample numbers 6 and 7 as comparative examples under the condition of 100°C is "86 W / m·K" and "63 W / m·K", respectively. In addition, regarding the thermal conductivity under the condition of 200°C, sample number 1 is "55 W / m·K", sample number 2 is "57 W / m·K", sample number 3 is "49 W / m·K", sample number 4 is "42 W / m·K", sample number 5 is "47 W / m·K", and sample number 8 is "44 W / m·K". In addition, the thermal conductivities of the samples No. 6 and No. 7 as comparative examples at 100° C. are “62 W / m·K” and “45 W / m·K”, respectively.

[0044] Thus, it can be seen that the samples No. 1 to No. 5 and No. 8 as examples of the present invention can maintain high thermal conductivity even in a high temperature environment. That is, the samples No. 1 to No. 5 and No. 8 as examples can maintain high heat dissipation in a high temperature environment and are therefore suitable for use in a high temperature environment.

[0045] The thermal conductivity of sample No. 6 as a comparative example at 100°C is higher than that of sample Nos. 1 to 5 and 8 as examples. The thermal conductivity of sample No. 7 as a comparative example at 100°C is higher than that of sample No. 5 as an example.

[0046] However, the reduction rate ((RT-100) / RT) of sample No. 6 and No. 7 is 30%, and the change rate of the thermal conductivity of the material is large when the temperature changes from room temperature (RT, 25°C) to 100°C. Therefore, for example, when a power element is set on a substrate made using sample No. 6 and No. 7, the temperature change rate of the power element itself may increase when the power element is driven. In that case, the stable drive of the power element is damaged, the output value of the power module is prone to deviation, and stable operation becomes difficult.

[0047] On the other hand, compared with sample number 6, the thermal conductivity of sample numbers 1 to 5 at each temperature such as room temperature, 100°C, and 200°C is lower, but since the change rate of thermal conductivity from room temperature to 100°C and from room temperature to 200°C is small, stable driving of the power element and stable operation of the power module can be expected.

[0048] Furthermore, since the fracture toughness of samples No. 1 to No. 5 is higher than that of samples No. 6 and No. 7, the probability of damage caused by temperature change of the power element itself is lower.

[0049] (Fracture toughness)

[0050] The fracture toughness of samples No. 1 to No. 5 and No. 8 was measured by the indentation fracture (IF) method. The fracture toughness measurement was carried out in accordance with JIS R1607-1995. A Vickers indenter was pressed into the mirror-polished test piece, and the fracture toughness was measured based on the indentation and crack length. The indentation load was 98 N (= 10 kgf) and the indentation time was 15 seconds.

[0051] As shown in Table 6, for the fracture toughness of samples No. 1 to No. 5 and No. 8, sample No. 1 is “7.1 MPa·m 1 / 2 ", sample number 2 is "7.5MPa·m 1 / 2 ", sample number 3 is "7.3MPa·m 1 / 2 ", sample number 4 is "6.7MPa·m 1 / 2 ", sample number 5 is "6.5MPa·m 1 / 2 ", sample number 8 is "6.2MPa·m 1 / 2 ". Sample No. 6 is "6.3MPa·m 1 / 2 ", sample number 7 is "6.4MPa·m 1 / 2 ”.

[0052] (Insulation Withstand Voltage)

[0053] The dielectric withstand voltage was measured for Sample Nos. 1 to 5 and Sample No. 8. The dielectric withstand voltage was measured by forming brass electrodes on the upper and lower surfaces of a substrate having a thickness of 0.32 mm and applying a voltage between the electrodes.

[0054] As shown in Table 6, the dielectric strength voltages of samples No. 1 to No. 5 and No. 8 are "12 kV" for sample No. 1, "12 kV" for sample No. 2, "11 kV" for sample No. 3, "10 kV" for sample No. 4, "11 kV" for sample No. 5, and "11 kV" for sample No. 8. In addition, the dielectric strength voltages of samples No. 6 and No. 7 as comparative examples are "11 kV" and "11 kV", respectively.

[0055] (Three-point bending strength)

[0056] About sample Nos. 1 to 5 and 8, three-point bending strength at room temperature based on JIS R1601 was measured.

[0057] As shown in Table 6, the three-point bending strength of Sample Nos. 1 to 5 and 8 is "613 MPa" for Sample No. 1, "602 MPa" for Sample No. 2, "604 MPa" for Sample No. 3, "534 MPa" for Sample No. 4, "521 MPa" for Sample No. 5, and "748 MPa" for Sample No. 8. In addition, the three-point bending strengths of Sample Nos. 6 and 7 as comparative examples are "716 MPa" and "600 MPa" respectively.

[0058] As described above, it is understood that Samples No. 1 to No. 5 and No. 8, which are Examples of the present invention, have excellent magnetic properties.

[0059] As described above, the silicon nitride sintered body of this embodiment contains silicon nitride particles (for example, SiN) and yttrium silicon oxynitride particles (Y6Si 11 N 20 O particles and YSi3O3N4 particles). In addition, the porosity of the silicon nitride sintered body is 14% or less. Therefore, according to the silicon nitride sintered body of the embodiment, a silicon nitride sintered body more suitable for use in a high temperature environment is provided.

[0060] It should be understood that all aspects of the embodiments disclosed in the present invention are exemplary rather than restrictive. In fact, the above-mentioned embodiments can be implemented in a variety of ways. In addition, without departing from the scope of the attached rights and their intentions, the above-mentioned embodiments can also be omitted, replaced, and changed in various ways.

Claims

1. A silicon nitride sintered body, wherein: It contains silicon nitride particles and yttrium silicon oxynitride particles. The porosity is 14% or less.

2. The silicon nitride sintered body according to claim 1, wherein The yttrium silicon oxynitride particles contain Y6Si 11 N 20 At least one of O particles, YSi3O3N4 particles, Y4Si2O7N2 particles and Y2Si3O3N4 particles.

3. The silicon nitride sintered body according to claim 2, wherein: The yttrium silicon oxynitride particles contain Y6Si 11 N 20 Two of the particles among O particles, YSi3O3N particles, Y4Si2O7N2 particles and YSi3O3N4 particles.

4. The silicon nitride sintered body according to claim 3, wherein: The Y6Si 11 N 20 The volume ratio of O particles / the YSi3O3N4 particles is greater than 1.

4.

5. The silicon nitride sintered body according to claim 4, wherein: The Y6Si 11 N 20 The volume ratio of O particles / the YSi3O3N4 particles is greater than 2.

0.

6. The silicon nitride sintered body according to claim 5, wherein: The Y6Si 11 N 20 The volume ratio of O particles / the YSi3O3N4 particles is greater than 3.

0.

7. The silicon nitride sintered body according to any one of claims 1 to 6, wherein Fracture toughness: 6.5MPa·m 1 / 2 above, The insulation withstand voltage is above 10kV. The three-point bending strength is above 521 MPa.

Citation Information

Patent Citations

  • Heating tube for metal molten immersion

    CN107324814A

  • Silicothermic reduction method for improving thermal conductivity and mechanical properties of silicon nitride ceramic substrate material

    CN112142476A

  • Silicon nitride sintered body

    TW201708162A

  • Silicon nitride sintered material method for manufacturing the same molten-metal-resistant member and wear resistant member formed from the same