An ultrafine cemented carbide tool with a high entropy alloy binder phase and a preparation method thereof
High-entropy alloy powder is prepared through high-temperature smelting-vacuum air atomization method and mixed with ultrafine tungsten carbide or rhenium solid solution, and the sintering process is optimized, which solves the problem of insufficient hardness and wear resistance in high-temperature cutting processing of cemented carbide tools. , realizes ultra-fine carbide cutting tools with high hardness, high toughness and strength, suitable for industrial production.
Patent Information
- Application Number
- CN202411382978.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-30
AI Technical Summary
Existing cemented carbide tools are prone to plastic deformation and chemical wear when processing difficult-to-process materials. The high-entropy alloys used contain high chemical activity elements such as Fe, Al, Cu, Sn, which leads to insufficient hardness and high-temperature wear resistance. , and low plasma sintering efficiency is not conducive to industrial production.
Ultrafine cemented carbide tool with high entropy alloy bonding phase is used to prepare high entropy alloy powder by high-temperature smelting-vacuum air atomization method. Combined with the optimized sintering process, high melting points are used to use Co, Er, Cr, W, Ru, The high-entropy alloys with Os and other elements form body-centered cubic and face-centered cubic phases as bonding phases, mixed with ultrafine tungsten carbide or tungsten carbide rhenium solid solution hard phases, ball milling and spray granulation, optimize sintering conditions to improve hardness and toughness.
The high hardness, toughness and strength of cemented carbide tools have been achieved, and the anti-collapse and wear resistance in high-temperature cutting processing has been improved. The hardness is ≥1900HV20, the fracture toughness is ≥13.0MPa·m1/2, and the bending strength is ≥4600MPa , suitable for industrial mass production.
Smart Images

Figure CN118875287B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cemented carbide manufacturing, and specifically relates to an ultrafine cemented carbide tool with a high entropy alloy bonding phase and a preparation method thereof. Background Art
[0002] High-temperature alloys and hardened steels usually contain hard phases and have high hardness. The high temperature and high pressure generated during the cutting process cause abrasive wear, adhesive wear and diffusion wear on the cutting tool. Therefore, processing these materials requires higher high-temperature hardness, strength and wear resistance of the cutting tool. Currently, fine-grained WC-Co hardness alloys, PCBN, PCD, etc. are mainly used in the field of high-temperature alloy finishing; fine-grained or ultra-fine-grained WC-Co hardness alloys are mainly used for rough machining of hardened steel, and PCBN, PCD, etc. are used for finishing. Due to their high brittleness, superhard materials such as PCBN and PCD are not as widely adaptable to working conditions as WC-Co hardness alloy coated tools.
[0003] At present, the binder phase of fine-grained or ultrafine-grained WC-Co hard alloy is mainly cobalt and cobalt alloy doped with elements such as Ru, Re, and Cr. The high-temperature hardness of cemented carbide using pure cobalt as the binder phase is low, which cannot meet the requirements of high-temperature wear resistance of cutting tools for high-temperature alloys and hardened steels; the toughness and high-temperature hardness of cemented carbide with doped binder phase are improved to a certain extent, but when facing severe working conditions such as continuous high-temperature cutting (for example, the tip temperature is higher than 800°C), the tool life is reduced due to the phase change of cobalt at high temperature. In order to ensure the hardness of cemented carbide, inhibitors such as VC are usually added to control the abnormal growth of WC grains in WC-Co cemented carbide. This method is easy to cause the strength of cemented carbide to decrease due to the aggregation of additives. In order to expand the scope of use of cemented carbide tools, cemented carbide with high entropy alloy as the binder phase has been studied and applied to a certain extent.
[0004] The Chinese patent application with publication number CN108060322A discloses a hard high entropy alloy composite material with three or more elements of Fe, Co, Ni, Cr, and Mn as the matrix, WC, BN, and diamond powder as the reinforcement phase, and a preparation method thereof using spark plasma sintering. The obtained hard high entropy composite material has good elongation and fracture toughness, but because the metal is the matrix and the hard phase is the reinforcement phase, the hardness of the alloy is only 960HV at most, which is much lower than the hard alloy with WC as the hard phase. In addition, the method uses plasma spark sintering with high cost, which is not conducive to industrial scale production.
[0005] The Chinese patent application with publication number CN109371307A discloses a method for preparing WC-based cemented carbide using high entropy alloy powder as a binder. High entropy alloy powder is obtained by mechanically alloying Fe, Co, Cr, Ni, Al, V, Ti, Cu, Zr, and Mn through high-energy ball milling, and then mixing with WC powder through ball milling, pressing and sintering to obtain cemented carbide. It is easy to obtain cemented carbide with target composition, but mechanical alloying easily causes alloy inclusions and leads to a decrease in the strength of cemented carbide.
[0006] The Chinese patent application with publication number CN113430443A discloses a method for preparing an ultrafine WC cemented carbide, wherein the bonding phase is a high entropy alloy composed of at least five of the elements Al, Nb, Ti, Zr, Ge, Si, V, Ta, Cr, Mn, Ce, Mo, W, and Hf without Co. The hard phase is submicron WC and other carbides and borides. The high entropy alloy is smelted into a bulk metal and then mechanically crushed into powder. Then, the cemented carbide is obtained by ball milling, pressing and sintering. The disadvantage is that elements such as Al, Ge, and Ce with low melting points are used, which easily reduces the high temperature wear resistance of the cemented carbide. Moreover, the method for preparing high entropy alloys by this method has a long process flow, which reduces production efficiency and increases the loss of high entropy alloy powder.
[0007] The US patent application with publication number US20240141461A1 discloses a sintered cemented carbide containing high entropy carbide and a binder phase. The binder phase is Co, Co-Ru, Ni, Co-Ni, Co-Ni-Cr, Co-Re, Co-Ni-Re, Co-Ni-Ru or a high entropy alloy, and the high entropy alloy composition is selected from four to ten kinds of Al, Be, Fe, Co, Cr, Ni, Cu, W, V, Zr, Ti, Mn, Hf, Nb, Mo, Ru, Re, Ge, Sn, C, B, Si. The high entropy carbide is sintered by spark plasma or discharge plasma after ball milling and mixing. The elements of the carbide are selected from at least one or four or five of W, Zr, V, Ti, Ta, Nb, Mo, Hf carbides, and the high entropy carbide can have BCC, FCC, HCP phases. It uses highly chemically active elements such as Al and Sn with low melting points. When processing difficult-to-process materials, the tool generates a large amount of heat, which will aggravate the chemical wear of the tool. In addition, elements such as Al and Sn are easy to volatilize and pollute the furnace cavity during industrial vacuum sintering. Moreover, the high entropy carbide of this invention adopts plasma sintering with low efficiency, which is also not conducive to industrial production.
[0008] In summary, carbide tools are prone to plastic deformation and chemical wear when machining difficult-to-machine materials, requiring tools to have higher high-temperature hardness and strength. The high chemical activity of Fe, Al, Cu, Sn, etc. easily leads to chemical wear, and the low melting points of these elements determine that the melting point of high-entropy alloys is relatively lower. Therefore, using carbide tools containing high-entropy alloys of these elements as a binder phase to machine difficult-to-machine materials is not the most ideal choice. Summary of the invention
[0009] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide an ultrafine cemented carbide tool with a high entropy alloy binder phase and a preparation method thereof.
[0010] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:
[0011] An ultrafine cemented carbide tool with a high entropy alloy binder phase comprises an ultrafine cemented carbide substrate, wherein the ultrafine cemented carbide substrate has a hard phase and a binder phase, wherein the hard phase is composed of ultrafine tungsten carbide or tungsten carbide-rhenium solid solution, and the binder phase is composed of a high-entropy alloy with a high melting point;
[0012] High entropy alloys are composed of ME1 and ME2 elements;
[0013] Wherein, the ME1 element is composed of Co and Er, and the atomic ratio of Co to Er is (1-2):1;
[0014] Among them, the ME2 elements include at least three of Cr, W, Ru and Os.
[0015] As a preferred embodiment of the ultrafine cemented carbide tool with a high entropy alloy binder phase described in the present invention, in the ultrafine cemented carbide matrix, the binder phase accounts for 4 to 12 wt%, and the hard phase accounts for 88 to 96 wt%.
[0016] As a preferred embodiment of the ultrafine cemented carbide tool with a high entropy alloy binder phase described in the present invention, the atomic percentage of each element in the ME1 element in the high entropy alloy is 10-35%, and the atomic percentage of each element in the ME2 element in the high entropy alloy is 5-30%.
[0017] As a preferred embodiment of the ultrafine cemented carbide tool with a high entropy alloy binder phase described in the present invention, the crystal structure of the high entropy alloy binder phase is mainly body-centered cubic phase (BCC) and face-centered cubic phase (FCC).
[0018] As a preferred embodiment of the ultrafine cemented carbide tool with a high entropy alloy binder phase described in the present invention, the average intercept length of the hard phase is 0.1 to 0.35 μm, and the intercept distribution of the hard phase conforms to the normal distribution.
[0019] As a preferred embodiment of the ultrafine cemented carbide tool with a high entropy alloy binder phase described in the present invention, the XRD diffraction (100) peak of the hard phase is the strongest, and the ratio of the intensity ratio of the (001) peak to the (100) peak is ≥0.50.
[0020] As a preferred embodiment of the ultrafine cemented carbide tool with a high entropy alloy binder phase described in the present invention, the liquidus temperature of the ultrafine cemented carbide substrate is ≥1430°C.
[0021] As a preferred embodiment of the ultrafine cemented carbide tool with a high entropy alloy binder phase described in the present invention, the ultrafine cemented carbide tool has a hardness of ≥1900 HV20 and a fracture toughness of ≥13.0 MPa·m 1 / 2 , flexural strength ≥4600MPa.
[0022] As a preferred embodiment of the ultrafine cemented carbide tool with a high entropy alloy binder phase described in the present invention, the friction coefficient of the ultrafine cemented carbide substrate is 0.1 to 0.3.
[0023] To solve the above technical problem, according to another aspect of the present invention, the present invention provides the following technical solution:
[0024] A method for preparing the above-mentioned ultrafine cemented carbide tool having a high entropy alloy binder phase comprises the following steps:
[0025] S1. Preparation of high entropy alloy powder: weighing ME1 and ME2 element powders required for high entropy alloy, melting them under high temperature conditions until they form a liquid state and ensuring that all elements are evenly dispersed; then, removing impurities from the melted liquid alloy, and using a vacuum gas atomization granulation process to make the liquid alloy after impurities removal into spherical or nearly spherical high entropy alloy powder;
[0026] S2. Mixing and forming of ultrafine cemented carbide: according to the composition of the ultrafine cemented carbide matrix, the bonding and hard phases are weighed, and added into a ball mill together with an appropriate amount of a molding agent and a ball milling medium, and ball milled and mixed until the mixture is uniform; then the mixed material is subjected to a spray granulation treatment to form particles suitable for pressing, and the particles are pressed and formed to obtain a blade green body;
[0027] S3, heat treatment and sintering of the blade green body: in a vacuum environment, the blade green body is heated to a temperature below 600°C to remove the forming agent; then the green body is heated to 800-1000°C in a carbon atmosphere for deoxidation treatment, and then sintered at 1480-1600°C for 1-2 hours to obtain a blade blank;
[0028] S4. Edge treatment and coating: The sintered blade blank is subjected to edge passivation treatment, and a coating is applied on the surface of the blank to obtain an ultrafine cemented carbide tool with a high entropy alloy bonding phase.
[0029] The beneficial effects of the present invention are as follows:
[0030] The present invention provides an ultrafine cemented carbide tool with a high entropy alloy binder phase and a preparation method thereof. The high entropy alloy powder is prepared by high temperature melting-vacuum gas atomization method, and the high entropy alloy powder is used as a binder phase. The optimized sintering process is used to promote the refinement of WC grains and the preferred orientation of the (001) crystal plane during WC recrystallization during sintering, thereby improving the hardness of the cemented carbide. The cemented carbide tool prepared by the present invention has the characteristics of high hardness, high toughness, and high strength, so that the tool exhibits good anti-breakage ability, high wear resistance and stability in the process of cutting and processing difficult-to-process materials such as high-temperature alloys. The hardness of the ultrafine cemented carbide tool is ≥1900HV20, and the fracture toughness is ≥13.0MPa·m 1 / 2 , the flexural strength is ≥4600MPa, the production cost of the invention is low, and it is suitable for industrial mass production. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0032] Figure 1 This is the microstructure diagram of the cemented carbide tool of Example 1.
[0033] Figure 2 This is the diffraction pattern of the hard phase of the cemented carbide tool of Example 1.
[0034] Figure 3 This is the microstructure diagram of the cemented carbide tool of Comparative Example 1.
[0035] Figure 4 This is the diffraction pattern of the hard phase of the cemented carbide tool of Comparative Example 1.
[0036] Figure 5This is the microstructure diagram of the cemented carbide tool of Comparative Example 2.
[0037] Figure 6 This is the microstructure diagram of the cemented carbide tool of Example 2.
[0038] Figure 7 This is the microstructure diagram of the cemented carbide tool of Comparative Example 3.
[0039] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0040] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] The invention provides an ultrafine cemented carbide tool with a high entropy alloy bonding phase and good anti-breakage ability, high wear resistance and stability, and a preparation method thereof.
[0042] The study found that the ultrafine cemented carbide prepared by high-entropy alloy powder containing at least three of the four elements Cr, W, Ru, and Os and high-entropy alloys of Co and Er as the binder phase not only has high high-temperature hardness, but also has good strength and toughness. After using this high-entropy alloy as a binder phase and mixing it with hard phases such as fine particles of WC, combined with an optimized sintering process, the WC grain refinement and the preferred orientation of the (001) crystal plane during WC recrystallization during sintering are promoted, and the hardness of the cemented carbide is improved. The addition of Er promotes the diffusion of each element, and combined with high-temperature melting and alloying, the distribution uniformity of each element in the high-entropy alloy is improved, thereby enhancing the high-entropy effect of the alloy and improving the strength and toughness of the cemented carbide prepared with this high-entropy alloy powder. Moreover, Er can remove impurities such as O, S, and P, purify the alloy grain boundaries, and reduce the probability of intergranular fracture of cemented carbide tools, thereby improving the alloy strength and tool life. In addition, Er improves the self-lubrication and corrosion resistance of cemented carbide tools during cutting.
[0043] According to one aspect of the present invention, the present invention provides the following technical solution:
[0044] An ultrafine cemented carbide tool with a high entropy alloy binder phase comprises an ultrafine cemented carbide substrate, wherein the ultrafine cemented carbide substrate has a hard phase and a binder phase, wherein the hard phase is composed of ultrafine tungsten carbide or tungsten carbide-rhenium solid solution, and the binder phase is composed of a high-entropy alloy with a high melting point;
[0045] High entropy alloys are composed of ME1 and ME2 elements;
[0046] Among them, the ME1 element is composed of Co and Er, and the atomic ratio of Co and Er is (1-2):1. In order to reduce the oxygen content in the powder, Co and Er preferably use Co-Er alloy powder;
[0047] Among them, the ME2 elements include at least three of Cr, W, Ru and Os.
[0048] Preferably, in the ultrafine cemented carbide matrix, the binder phase accounts for 4 to 12 wt %, and the hard phase accounts for 88 to 96 wt %.
[0049] Preferably, the hard phase has a Fisher grain size of 0.1 to 0.6 μm.
[0050] Preferably, the atomic percentage of each element in the ME1 elements in the high entropy alloy is 10-35%, and the atomic percentage of each element in the ME2 elements in the high entropy alloy is 5-30%.
[0051] Further preferably, the ME2 element consists of Cr, W, Ru and Os, and the atomic percentages of Co, Er, Cr, W, Ru and Os in the high entropy alloy are 20-35%, 15-30%, 15-30%, 5-15%, 5-15% and 5-15%, respectively;
[0052] Further preferably, the ME2 elements consist of Cr, W and Os, and the atomic percentages of Co, Er, Cr, W and Os in the high entropy alloy are 25-35%, 25-30%, 25-30%, 5-10% and 5-10%, respectively.
[0053] Preferably, the crystal structure of the high entropy alloy binder phase is mainly body-centered cubic phase (BCC) and face-centered cubic phase (FCC).
[0054] Preferably, the average intercept length of the hard phase is 0.1-0.35 μm, and the intercept distribution of the hard phase conforms to a normal distribution.
[0055] Preferably, the XRD diffraction (100) peak of the hard phase is the strongest, and the intensity ratio of the (001) peak to the (100) peak is ≥0.50.
[0056] Preferably, the liquidus temperature of the ultrafine cemented carbide substrate is ≥1430°C.
[0057] Preferably, the hardness of the ultrafine cemented carbide tool is ≥1900HV20 and the fracture toughness is ≥13.0MPa·m 1 / 2 , flexural strength ≥4600MPa.
[0058] Preferably, the friction coefficient of the ultrafine cemented carbide substrate is 0.1 to 0.3.
[0059] According to another aspect of the present invention, the present invention provides the following technical solution:
[0060] A method for preparing the above-mentioned ultrafine cemented carbide tool having a high entropy alloy binder phase comprises the following steps:
[0061] S1. Preparation of high entropy alloy powder: weighing ME1 and ME2 element powders required for high entropy alloy, melting them under high temperature conditions until they form a liquid state and ensuring that all elements are evenly dispersed; then, removing impurities from the melted liquid alloy, and using a vacuum gas atomization granulation process to make the liquid alloy after impurities removal into spherical or nearly spherical high entropy alloy powder;
[0062] S2. Mixing and forming of ultrafine cemented carbide: according to the composition of the ultrafine cemented carbide matrix, the bonding and hard phases are weighed, and added into a ball mill together with an appropriate amount of carbon powder, a forming agent and a ball milling medium, and ball milled and mixed until the mixture is uniform; then the mixed material is subjected to spray granulation treatment to form particles suitable for pressing, and the particles are pressed and formed to obtain a blade blank;
[0063] S3, heat treatment and sintering of the blade green body: in a vacuum environment, the blade green body is heated to a temperature below 600°C to remove the forming agent; then the green body is heated to 800-1000°C in a carbon atmosphere for deoxidation treatment, and then sintered at 1480-1600°C for 1-2 hours to obtain a blade blank;
[0064] S4. Edge treatment and coating: The sintered blade blank is subjected to edge passivation treatment, and a coating is applied on the surface of the blank to obtain an ultrafine cemented carbide tool with a high entropy alloy bonding phase.
[0065] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0066] Example 1
[0067] A method for preparing an ultrafine cemented carbide tool having a high entropy alloy binder phase comprises the following steps:
[0068] S1. Preparation of high entropy alloy powder: Co-Er, Cr, W, Ru metal powders were weighed, and the atomic percentages of Co, Er, Cr, W, and Ru were 35:25:30:5:5. The weighed powders were melted into liquid alloys at high temperature, and then impurities were removed, and the content of each element was detected. Then vacuum gas atomization granulation was used to obtain spherical or nearly spherical high entropy alloy powders with a Fisher particle size of <50μm. The XRD diffraction method detected that the crystal structure of the high entropy alloy binder phase was mainly body-centered cubic phase (BCC) and face-centered cubic phase (FCC), with a small amount of hexagonal phase (HCP);
[0069] S2. Mixing and molding of ultrafine cemented carbide: weigh 10% by mass of high entropy alloy powder, 90% by mass of WReC (Re accounts for 5% of the total atomic weight of W+Re, and the Fisher particle size is 0.4-0.6 μm), a trace amount of carbon powder, a molding agent, and a ball milling medium, add them into a ball mill for ball milling, spray dry after ball milling, and press to obtain a blade green body;
[0070] S3. Heat treatment and sintering of the blade green body: In a vacuum environment, heat the blade green body to a temperature below 600°C to remove the forming agent; then heat the green body to 1000°C in a carbon atmosphere for deoxidation, and then sinter at 1480°C for 2 hours to obtain a blade blank; crush part of the prepared blade blank into powder, and use differential thermal analysis to measure the liquid phase starting temperature of the cemented carbide powder to be 1430°C. Polish the prepared cemented carbide tool to a mirror surface, and use GH4169 high-temperature alloy as the friction pair material, and the friction coefficient is measured to be 0.21. The electrolytic method is used to remove the bonding phase of the cemented carbide, and the XRD diffraction method is used to detect the WC diffraction peak as shown Figure 2 As shown, the (100) peak is the strongest, and the intensity ratio of the (001) peak to the (100) peak is 0.51.
[0071] S4. Edge treatment and coating: The sintered blade blank is subjected to edge passivation treatment, and a TiAlZrN superhard coating is coated on the surface of the blank using a PVD method to obtain an ultrafine cemented carbide tool with a high entropy alloy bonding phase.
[0072] The microstructure of the ultrafine cemented carbide tool with high entropy alloy binder phase prepared in this embodiment (such as Figure 1 The average intercept length of the tungsten carbide phase was found to be 0.35 μm. The following parameters were measured for its performance: hardness of 1906 HV20, bending strength of 5016 MPa, and fracture toughness of 14.2 MPa·m 1 / 2 .
[0073] Comparative Example 1
[0074] The difference from Example 1 is that the cemented carbide ingredient is Co 0.35 Fe 0.25 Cr 0.3 Mn 0.05 Ru 0.05 The high entropy alloy powder is substituted for the high entropy alloy powder of Example 1, and the microstructure of the ultrafine cemented carbide tool with a high entropy alloy binder phase is as follows: Figure 3 As shown, the average intercept length of the tungsten carbide phase was measured to be 0.58 μm. The performance was tested and the following parameters were measured: friction coefficient was 0.32, hardness was 1863 HV20, bending strength was 4501 MPa, and fracture toughness was 11.68 MPa·m 1 / 2 The XRD diffraction results of the hard phase are as follows: Figure 4 As shown, the intensity ratio of the (001) peak to the (100) peak was measured to be 0.49.
[0075] Comparative Example 2
[0076] The difference from Example 1 is that the cemented carbide ingredients use Co powder instead of the high entropy alloy powder of Example 1, and the microstructure of the obtained cemented carbide tool is as follows: Figure 5 As shown, there are abnormally grown coarse particles. The average intercept length of the tungsten carbide phase is 0.6μm. The performance is tested and the following parameters are measured: the friction coefficient is 0.45, the liquid phase starting temperature of the cemented carbide powder is 1285℃, the hardness is 1728HV20, the bending strength is 4136MPa, and the fracture toughness is 11.26MPa·m 1 / 2 The binder phase of cemented carbide was removed by electrolysis, and WC diffraction peaks were detected by XRD diffraction. The (100) peak was the strongest, and the intensity ratio of the (001) peak to the (100) peak was 0.45.
[0077] The tools prepared in Example 1 and Comparative Examples 1-2 were used to perform high-speed turning of GH4169 bar material, with blade type: CNMG 120408E-SC3, VC=90m / min, f=0.1mm / rev, ap=1.0mm, and wet cutting. The test results are shown in Table 1. Comparative Example 1-2 showed severe built-up edge on the tool tip.
[0078] Table 1
[0079]
[0080] Example 2
[0081] A method for preparing an ultrafine cemented carbide tool having a high entropy alloy binder phase comprises the following steps:
[0082] S1. Preparation of high entropy alloy powder: Co-Er, Cr, W, Os metal powders were weighed, and the atomic percentages of Co, Er, Cr, W, and Os were 35:20:30:5:10. The weighed powders were melted into liquid alloys at high temperature, and then impurities were removed, and the content of each element was detected. Then vacuum gas atomization granulation was used to obtain spherical or nearly spherical high entropy alloy powders with a Fisher particle size of <50μm. The XRD diffraction method detected that the crystal structure of the high entropy alloy binder phase was mainly body-centered cubic phase (BCC) and face-centered cubic phase (FCC), with a small amount of hexagonal phase (HCP);
[0083] S2. Mixing and molding of ultrafine cemented carbide: weigh 7% by mass of high entropy alloy powder, 93% by mass of WC (Fischer particle size of 0.2-0.4 μm), trace carbon powder, molding agent, and ball milling medium, add them into a ball mill for ball milling, spray dry after ball milling, and press to obtain a blade green body;
[0084] S3. Heat treatment and sintering of the blade blank: In a vacuum environment, the blade blank is heated to a temperature below 600°C to remove the forming agent; then the blank is heated to 900°C in a carbon atmosphere for deoxidation, and then sintered at 1500°C for 2 hours to obtain a blade blank; the prepared cemented carbide tool is polished to a mirror surface, and the friction coefficient is measured to be 0.18 using GH4169 high-temperature alloy as the friction pair material. Part of the prepared blade blank is crushed into powder, and the liquid phase starting temperature of the cemented carbide powder is measured to be 1508°C by differential thermal analysis. The bonding phase of the cemented carbide is removed by electrolysis, and the WC diffraction peak is detected by XRD diffraction. The (100) peak is the strongest, and the intensity ratio of the (001) peak to the (100) peak is 0.56.
[0085] S4. Edge treatment and coating: The sintered blade blank is subjected to edge passivation treatment, and an Al2O3-TiAlN superhard coating is coated on the surface of the blank using a CVD method to obtain an ultrafine cemented carbide tool with a high entropy alloy bonding phase.
[0086] The microstructure of the ultrafine cemented carbide tool with high entropy alloy binder phase prepared in this embodiment (such as Figure 6 The average intercept length of the tungsten carbide phase was found to be 0.26 μm. The following parameters were measured for its performance: hardness of 2106 HV20, bending strength of 4601 MPa, fracture toughness of 13.1 MPa·m 1 / 2 .
[0087] Comparative Example 3
[0088] The difference from Example 2 is that the cemented carbide ingredients use Co powder instead of the high entropy alloy powder of Example 2, add 0.5% by mass of Cr3C2, and the balance is WC. The microstructure of the obtained cemented carbide tool is as follows: Figure 7 As shown, some tungsten carbide particles grow significantly, and the average intercept length of the tungsten carbide phase is 0.4μm. The performance is tested and the following parameters are measured: the liquid phase starting temperature of the cemented carbide powder is 1321℃, the friction coefficient is 0.39, the hardness is 1781HV20, the bending strength is 3902MPa, and the fracture toughness is 10.81MPa·m 1 / 2 The XRD diffraction results show that the intensity ratio of the (001) peak to the (100) peak is 0.43.
[0089] Example 3
[0090] A method for preparing an ultrafine cemented carbide tool having a high entropy alloy binder phase comprises the following steps:
[0091] S1. Preparation of high entropy alloy powder: Co-Er, Cr, W, Ru, Os metal powders were weighed, and the atomic percentages of Co, Er, Cr, W, Ru, and Os were 30:30:25:5:5:5. The weighed powders were melted into liquid alloys at high temperature, then impurities were removed, and the content of each element was detected. Then vacuum gas atomization granulation was used to obtain spherical or nearly spherical high entropy alloy powders with a Fisher particle size of <50μm. The XRD diffraction method detected that the crystal structure of the high entropy alloy binder phase was mainly body-centered cubic phase (BCC) and face-centered cubic phase (FCC), with a small amount of hexagonal phase (HCP);
[0092] S2. Mixing and molding of ultrafine cemented carbide: weigh 5% by mass of high entropy alloy powder, 95% by mass of WC (Fischer particle size of 0.1-0.3 μm), trace carbon powder, molding agent and ball milling medium, add them into a ball mill for ball milling, spray dry after ball milling, and press to obtain a blade green body;
[0093] S3, heat treatment and sintering of the blade green body: in a vacuum environment, the blade green body is heated to a temperature below 600°C to remove the forming agent; then the green body is heated to 800°C in a carbon atmosphere for deoxidation treatment, and then sintered at 1550°C for 2 hours to obtain a blade blank;
[0094] S4. Edge treatment and coating: The sintered blade blank is subjected to edge passivation treatment, and an Al2O3-TiAlN superhard coating is coated on the surface of the blank using a CVD method to obtain an ultrafine cemented carbide tool with a high entropy alloy bonding phase.
[0095] The microstructure of the ultrafine cemented carbide tool with a high entropy alloy binder phase prepared in this embodiment was studied, and the average intercept length of the tungsten carbide phase was measured to be 0.19 μm. The performance was tested and the following parameters were measured: friction coefficient of 0.16, hardness of 2306 HV20, bending strength of 4836 MPa, fracture toughness of 13.8 MPa·m 1 / 2 The XRD diffraction showed that the intensity ratio of the (001) peak to the (100) peak was 0.55.
[0096] Comparative Example 4
[0097] The difference from Example 3 is that the cemented carbide ingredient is Co 0.6 Cr 0.4 The high entropy alloy powder of Example 3 was replaced by Cr3C2 with a mass percentage of 0.5%, and the balance was WC. The WC-Cr3C2-Co cemented carbide obtained had an average intercept length of 0.37 μm for the tungsten carbide phase. The following parameters were measured when the properties were tested: friction coefficient of 0.46, hardness of 1894 HV20, bending strength of 4113 MPa, and fracture toughness of 10.92 MPa·m 1 / 2 The XRD diffraction results show that the intensity ratio of the (001) peak to the (100) peak is 0.44.
[0098] The present invention prepares high entropy alloy powder by high temperature melting-vacuum gas atomization method, uses this high entropy alloy powder as a binder phase, and cooperates with an optimized sintering process to promote WC grain refinement and the preferred orientation of the (001) crystal plane during WC recrystallization during sintering, thereby improving the hardness of cemented carbide. The cemented carbide tool prepared by the present invention has the characteristics of high hardness, high toughness, and high strength, so that the tool exhibits good anti-breakage ability, high wear resistance and stability in the process of cutting and processing difficult-to-process materials such as high-temperature alloys. The hardness of the ultrafine cemented carbide tool is ≥1900HV20, and the fracture toughness is ≥13.0MPa·m 1 / 2 , the flexural strength is ≥4600MPa, the production cost of the invention is low, and it is suitable for industrial mass production.
[0099] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. An ultrafine cemented carbide tool having a high entropy alloy binder phase, characterized in that: The ultrafine cemented carbide matrix comprises an ultrafine cemented carbide matrix having a hard phase and a binder phase, wherein the hard phase is composed of ultrafine tungsten carbide or tungsten carbide-rhenium solid solution, and the binder phase is composed of a high-entropy alloy with a high melting point; High entropy alloys are composed of ME1 and ME2 elements; Among them, the ME1 element is composed of Co and Er, and the atomic ratio of Co to Er is (1-2):1; The ME2 elements include at least three of Cr, W, Ru and Os.
2. The ultrafine cemented carbide tool with a high entropy alloy binder phase according to claim 1, characterized in that: In the ultrafine cemented carbide matrix, the binder phase accounts for 4 to 12 wt%, and the hard phase accounts for 88 to 96 wt%.
3. The ultrafine cemented carbide tool with a high entropy alloy binder phase according to claim 1, characterized in that: The atomic percentage of each element in the ME1 elements in the high entropy alloy is 10 to 35%, and the atomic percentage of each element in the ME2 elements in the high entropy alloy is 5 to 30%.
4. The ultrafine cemented carbide tool with a high entropy alloy binder phase according to claim 1, characterized in that: The crystal structure of the binder phase of high entropy alloys is mainly body-centered cubic phase and face-centered cubic phase.
5. The ultrafine cemented carbide tool with a high entropy alloy binder phase according to claim 1, characterized in that: The average intercept length of the hard phase is 0.1-0.35 μm, and the intercept distribution of the hard phase conforms to the normal distribution.
6. The ultrafine cemented carbide tool with a high entropy alloy binder phase according to claim 1, characterized in that: The XRD diffraction (100) peak of the hard phase is the strongest, and the intensity ratio of the (001) peak to the (100) peak is ≥0.
50.
7. The ultrafine cemented carbide tool with a high entropy alloy binder phase according to claim 1, characterized in that: The liquidus temperature of the ultrafine cemented carbide substrate is ≥1430°C.
8. The ultrafine cemented carbide tool with a high entropy alloy binder phase according to claim 1, characterized in that: The hardness of ultrafine carbide tools is ≥1900HV20, and the fracture toughness is ≥13.0MPa·m 1 / 2 , flexural strength ≥4600MPa.
9. The ultrafine cemented carbide tool with a high entropy alloy binder phase according to claim 1, characterized in that: The friction coefficient of the ultrafine cemented carbide substrate is 0.1 to 0.
3.
10. A method for preparing an ultrafine cemented carbide cutting tool having a high entropy alloy binder phase according to any one of claims 1 to 9, characterized in that: The steps include: S1. Preparation of high-entropy alloy powder: Weighing the ME1 and ME2 element powders required for the high-entropy alloy, melting them under high temperature conditions until they form a liquid and ensuring that the elements are evenly dispersed; then, removing impurities from the melted liquid alloy and forming the removed liquid alloy into spherical or nearly spherical high-entropy alloy powder using a vacuum gas atomization granulation process; S2. Mixing and forming ultrafine cemented carbide: According to the composition of the ultrafine cemented carbide matrix, the binder and hard phases are weighed, and added to a ball mill together with an appropriate amount of a forming agent and a ball milling medium, and ball milled until the mixture is uniform; the mixed material is then spray granulated to form particles suitable for pressing, and the particles are pressed into shape to obtain a blade green body; S3. Heat treatment and sintering of the blade green body: In a vacuum environment, the blade green body is heated to a temperature below 600°C to remove the forming agent; then the green body is heated to 800-1000°C in a carbon atmosphere for deoxidation treatment, and then sintered at 1480-1600°C for 1-2 hours to obtain a blade blank; S4. Edge treatment and coating: The sintered blade blank is subjected to edge passivation treatment, and a coating is applied on the surface of the blank to obtain an ultrafine cemented carbide tool with a high entropy alloy binder phase.
Citation Information
Patent Citations
Preparation method for hard high-entropy alloy composite material
CN108060322A
Preparation method of WC-based hard alloy with high-entropy powder as binder
CN109371307A
Preparation method of superfine WC hard alloy
CN113430443A
Cemented carbide containing muli-component high entropy carbide and / or multi-component high entropy alloy
US20240141461A1
Titanium carbonitride based metal ceramic based on high-entropy alloy binder phase and preparation method of metal ceramic
CN102787266A
Cited By
Superfine hard alloy cutter material for high-temperature material processing and preparation method of superfine hard alloy cutter material
CN119913409A
An ultra-fine cemented carbide cutting tool material for high-temperature material processing and its preparation method