Tantalum-containing PVD (Physical Vapor Deposition) hard coating and preparation method and equipment thereof
By preparing AlCrTaN coating, the problem of reduced wear resistance of the coating under high temperature environment is solved, the hardness and toughness are improved, the service life of the tool is extended, and it is suitable for a variety of matrix materials.
Patent Information
- Application Number
- CN202410983276.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-01
AI Technical Summary
The wear resistance of advanced cutting tools in high temperature environments has decreased, resulting in rapid failure of the tool. The existing tantalum-containing PVD hard coating and its preparation method have not been reported.
AlCrTaN coating is made of Al, Cr, Ta and N, and is prepared by arc deposition or magnetron + arc deposition method. It has a nanostructure structure, preferably components are 20-25% Cr, 5-10% Ta, 40- 45%N, hardness is 30-35GPa, friction coefficient is 0.5-0.6, elastic modulus is 400-530GPa, and binding force is 70-90N.
It significantly improves the wear resistance of the coating in high temperature environments and extends its service life. It is suitable for matrixes such as cemented carbide and bearing steel, and is suitable for tools and stamping abrasives.
Smart Images

Figure CN118880236A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of surface engineering, and in particular to a tantalum-containing PVD hard coating and a preparation method and equipment thereof. Background Art
[0002] In the field of advanced processing and manufacturing, the quality and stability of cutting tools are key factors in improving processing efficiency and quality, reducing production costs, and accelerating product research and development. As one of the three key technologies in this field, coating technology can effectively improve the surface hardness and wear resistance of cutting tools, thereby significantly improving cutting performance.
[0003] AlCrN is a widely used hard coating material with a hardness of over 30GPa. However, with the development of advanced cutting technology and the popularization and application of high-performance difficult-to-process materials, the tool surface is subjected to increasingly severe working conditions, and its edge temperature can even exceed 1000°C. High cutting temperature will directly lead to increased oxidation of the AlCrN coating and decreased wear resistance, resulting in rapid failure of the tool.
[0004] The present invention combines the advantages of the original coating to prepare a multi-component hard AlCrTaN coating with both high-temperature oxidation resistance and wear resistance, which is used to solve the problems of reduced wear resistance and shortened service life of tool coatings caused by high-temperature oxidation.
[0005] So far, PVD hard coating containing tantalum element and its preparation method have not been reported. Summary of the invention
[0006] The purpose of the present invention is to solve the above technical problems and propose a tantalum-containing PVD hard coating and a preparation method and equipment thereof. The AlCrTaN coating has high hardness, good toughness, and excellent resistance to high-temperature oxidation. It can significantly improve the wear resistance of the coating in a high-temperature environment, thereby increasing the service life of the coating.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] A tantalum-containing PVD hard coating comprises a substrate, on which a tantalum-containing PVD hard coating is arranged, wherein the tantalum-containing PVD hard coating comprises four elements: Al, Cr, Ta and N, and the tantalum-containing PVD hard coating is an AlCrTaN coating and the AlCrTaN coating has a nanostructure.
[0009] Preferably, the AlCrTaN coating comprises the following components in atomic percentage: 20-25% Cr, 5-10% Ta, 40-45% N, and the balance is Al.
[0010] Preferably, the thickness of the AlCrTaN coating is in the range of 2 to 4 μm, the AlCrTaN coating is composed of a Fcc-(Cr, Al)N phase, and the Ta element in the AlCrTaN coating replaces Al or Cr to form a solid solution phase.
[0011] Preferably, the hardness of the AlCrTaN coating is 30-35 GPa; the friction coefficient of the AlCrTaN coating is 0.5-0.6; the elastic modulus of the AlCrTaN coating is 400-530 GPa; and the bonding force of the AlCrTaN coating is 70-90N.
[0012] The present invention also discloses a novel method for preparing a tantalum-containing PVD hard coating, comprising the following steps:
[0013] Process 1: surface pretreatment of the substrate;
[0014] Process 2 is glow cleaning;
[0015] Process three is ion etching treatment;
[0016] Process four is the deposition of the AlCrTaN coating.
[0017] Preferably, the surface pretreatment of the substrate comprises first mechanically polishing the substrate, then ultrasonically cleaning the substrate in distilled water, acetone and alcohol in sequence, and drying the substrate for standby use.
[0018] Preferably, the glow cleaning is to fix the sample after surface pretreatment in a vacuum chamber so that the pressure of the chamber is maintained at 10 -4 Pa, and then argon gas is introduced for glow discharge to remove impurities on the sample surface.
[0019] Preferably, the ion etching treatment refers to using a pure Cr target to perform metal ion bombardment to remove surface impurities and increase film-substrate bonding strength.
[0020] Preferably, the deposition of the AlCrTaN coating includes two methods:
[0021] The first method is arc deposition: AlCrTa alloy target is used as arc target, N2 is used as reaction gas, and AlCrTaN coating is deposited. The specific parameters are as follows: deposition temperature is 300-500℃, target current is 50-100A, nitrogen flow rate is 100-300sccm, gas pressure is 1-3Pa, deposition bias is -80V to -140V, deposition time is 30-200min, the distance between substrate and target is 10-15cm, and sample rotation and revolution are carried out simultaneously;
[0022] The second method is magnetron + arc deposition: that is, AlCr alloy target is used as arc target and pure Ta target is used as magnetron target. In nitrogen atmosphere, magnetron sputtering Ta target and arc evaporation AlCr target are used to prepare AlCrTaN coating on the substrate surface. The specific parameters are as follows: deposition temperature is 300-500℃, nitrogen flow rate is 100-300sccm, gas pressure is 1-3Pa, deposition time is 30-200min, the distance between substrate and target is 10-15cm, arc target current is 50-100A, arc target deposition bias is -80V to -140V, and the average sputtering power of magnetron sputtering Ta target is 5-30W / cm 2 .
[0023] The present invention also discloses a preparation device for a tantalum-containing PVD hard coating, the preparation device comprising a base, on which a substrate surface treatment device, a glow cleaning device, an ion etching device and an AlCrTaN coating deposition device are installed, the substrate surface treatment device comprising a box body, a support plate is fixed in the box body, two electric push rods are fixed in the box body, the output end of the electric push rod is fixedly connected to a clamping plate that slides on the upper end of the support plate for clamping the substrate, a hydraulic cylinder is installed on the inner top of the box body, a moving plate is fixed on the output end of the hydraulic cylinder, two sleeves are fixed on the inner bottom of the box body, a sliding rod is slidably connected in the sleeve, and the The lower end of the sliding rod is fixedly connected to the upper end of the movable plate, and the bottom of the movable plate is fixedly connected to a changing box, and two bevel gears are meshed in the changing box, and the shaft ends of the two bevel gears are fixed with short rods, and the short rods penetrate the changing box and are rotatably connected thereto. A motor is installed on the changing box, and the output end of the motor is fixedly connected to the short rod, and the other short rod is fixedly connected to a polishing disk. A dust collecting box is installed on the inner bottom of the box body, and a fan is installed on the dust collecting box, and the air inlet end of the fan is connected to the dust collecting box, and a metal shaping hose is fixed on the dust collecting box, and a dust suction pipe is installed on the metal shaping hose, and a plurality of dust suction holes are penetrated through the dust suction pipe.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The present invention is a novel tantalum-containing PVD hard coating, which is composed of four elements: Al, Cr, Ta and N, and has a thickness of 1-4 μm. The present invention uses an arc coating device, or a method combining magnetron sputtering and arc to prepare the hard coating, and its composition is controllable, and the process is simple to operate.
[0026] 2. Compared with the prior art, the present invention can improve the high temperature oxidation resistance and hardness of the coating by adding Ta element to the aluminum-containing transition metal nitride AlCrN, thereby reducing the wear of the coating and increasing its service life.
[0027] 3. The AlCrTaN coating preparation process developed by the present invention has good repeatability. The prepared coating is suitable for substrates such as cemented carbide and bearing steel, and has broad application prospects in the fields of various cutting tools and stamping tools.
[0028] In summary, the AlCrTaN coating in the present invention has high hardness, good toughness, and excellent high-temperature oxidation resistance, and can significantly improve the wear resistance of the coating in a high-temperature environment, thereby increasing the service life of the coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The cross-sectional morphology of the AlCrTaN coating prepared under different bias voltages;
[0030] Figure 2 The mechanical properties test results of AlCrTaN coatings prepared under different bias voltages;
[0031] Figure 3 The friction coefficient test results of the AlCrTaN coating prepared under different bias voltages;
[0032] Figure 4 This is a schematic diagram of the structure of a preparation device for a tantalum-containing PVD hard coating proposed by the present invention;
[0033] Figure 5 The present invention provides a schematic structural diagram of a substrate surface treatment device in a tantalum-containing PVD hard coating preparation device.
[0034] In the figure: 1 base, 2 substrate surface treatment device, 3 glow cleaning device, 4 ion etching device, 5 AlCrTaN coating deposition device, 6 hydraulic cylinder, 7 sleeve, 8 sliding rod, 9 moving plate, 10 motor, 11 change box, 12 polishing disc, 13 dust suction pipe, 14 dust suction hole, 15 electric push rod, 16 clamping plate, 17 metal shaping hose, 18 dust collection box, 19 fan, 20 support plate. DETAILED DESCRIPTION
[0035] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0036] Reference Figure 1-Figure 5 A tantalum-containing PVD hard coating comprises a substrate, on which a tantalum-containing PVD hard coating is arranged, wherein the tantalum-containing PVD hard coating comprises four elements: Al, Cr, Ta and N, and the tantalum-containing PVD hard coating is an AlCrTaN coating and the AlCrTaN coating has a nanostructured structure.
[0037] In the present invention, the AlCrTaN coating comprises the following components in atomic percentage: 20-25% Cr, 5-10% Ta, 40-45% N, and the balance is Al.
[0038] Preferably, the thickness of the AlCrTaN coating is in the range of 2 to 4 μm, the AlCrTaN coating is composed of a Fcc-(Cr, Al)N phase, and the Ta element in the AlCrTaN coating replaces Al or Cr to form a solid solution phase.
[0039] Preferably, the hardness of the AlCrTaN coating is 30-35 GPa; the friction coefficient of the AlCrTaN coating is 0.5-0.6; the elastic modulus of the AlCrTaN coating is 400-530 GPa; and the bonding force of the AlCrTaN coating is 70-90N.
[0040] The present invention also discloses a novel method for preparing a tantalum-containing PVD hard coating, comprising the following steps:
[0041] Process 1: surface pretreatment of the substrate;
[0042] Process 2 is glow cleaning;
[0043] Process three is ion etching treatment;
[0044] Process four is the deposition of the AlCrTaN coating.
[0045] Preferably, the surface pretreatment of the substrate comprises first mechanically polishing the substrate, then ultrasonically cleaning the substrate in distilled water, acetone and alcohol in sequence, and drying the substrate for standby use.
[0046] Preferably, the glow cleaning is to fix the sample after surface pretreatment in a vacuum chamber so that the pressure of the chamber is maintained at 10 -4 Pa, and then argon gas is introduced for glow discharge to remove impurities on the sample surface.
[0047] Preferably, the ion etching treatment refers to using a pure Cr target to perform metal ion bombardment to remove surface impurities and increase film-substrate bonding strength.
[0048] Preferably, the deposition of the AlCrTaN coating includes two methods:
[0049] The first method is arc deposition: AlCrTa alloy target is used as arc target, N2 is used as reaction gas, and AlCrTaN coating is deposited. The specific parameters are as follows: deposition temperature is 300-500℃, target current is 50-100A, nitrogen flow rate is 100-300sccm, gas pressure is 1-3Pa, deposition bias is -80V to -140V, deposition time is 30-200min, the distance between substrate and target is 10-15cm, and sample rotation and revolution are carried out simultaneously;
[0050] The second method is magnetron + arc deposition: that is, AlCr alloy target is used as arc target and pure Ta target is used as magnetron target. In nitrogen atmosphere, magnetron sputtering Ta target and arc evaporation AlCr target are used to prepare AlCrTaN coating on the substrate surface. The specific parameters are as follows: deposition temperature is 300-500℃, nitrogen flow rate is 100-300sccm, gas pressure is 1-3Pa, deposition time is 30-200min, the distance between substrate and target is 10-15cm, arc target current is 50-100A, arc target deposition bias is -80V to -140V, and the average sputtering power of magnetron sputtering Ta target is 5-30W / cm 2 .
[0051] Example 1
[0052] In this embodiment, the substrate is made of YT15 cemented carbide, and the preparation method of the AlCrTaN coating is as follows:
[0053] Step 1: Grind and polish the cut cemented carbide material. After the cemented carbide substrate is polished to a mirror surface, ultrasonically clean the substrate with deionized water, acetone and alcohol in sequence, and then dry it for use.
[0054] Step 2: After the alloy is pretreated, it is fixed on the substrate rotating rack and placed in the deposition vacuum chamber so that the alloy sample is about 15 cm away from the target. The deposition chamber is evacuated to 5×10 -3 Pa, and then turn on the heating to make the chamber temperature reach 350°C; fill with argon gas, adjust the vacuum chamber pressure to 2Pa, and perform glow discharge plasma surface cleaning treatment for 30 minutes under a bias of -700V.
[0055] Step 3: After the argon ion bombardment, the argon gas flow rate was reduced to make the chamber pressure reach 0.8 Pa, and the ion etching treatment was performed at a bias voltage of -700 V and a Cr target current of 100 A for 10 min.
[0056] Step 4: Close the argon channel, open the nitrogen channel (reaction gas), and prepare the AlCrTaN coating in a pure N2 atmosphere. The relevant parameters are as follows: chamber pressure 1Pa, bias voltage -80V, AlCrTa target current 80A, rotation speed 5rpm, duty cycle 50%, frequency 20, and time 120min.
[0057] Example 2
[0058] The difference between this embodiment and embodiment 1 is that: during the deposition process (step 4), the AlCrTaN coating is prepared in a pure N2 atmosphere, and the relevant parameters are as follows: chamber pressure 1Pa, bias voltage -100V, AlCrTa target current 80A, rotation speed 5rpm, duty cycle 50%, frequency 20, time 120min.
[0059] Example 3
[0060] The difference between this embodiment and embodiment 1 is that: during the deposition process (step 4), the AlCrTaN coating is prepared in a pure N2 atmosphere, and the relevant parameters are as follows: chamber pressure 1Pa, bias voltage -120V, AlCrTa target current 80A, rotation speed 5rpm, duty cycle 50%, frequency 20, time 120min.
[0061] Example 4
[0062] The difference between this embodiment and embodiment 1 is that: during the deposition process (step 4), the AlCrTaN coating is prepared in a pure N2 atmosphere, and the relevant parameters are as follows: chamber pressure 1Pa, bias voltage -140V, AlCrTa target current 80A, rotation speed 5rpm, duty cycle 50%, frequency 20, time 120min.
[0063] pass Figure 1 The cross-sectional morphology of the AlCrTaN coatings prepared under different bias voltages shows that the coatings prepared under the four bias voltages are well bonded to the substrate without obvious cracking. In addition, the bias voltage affects the deposition thickness and microstructure of the coating.
[0064] pass Figure 2 The mechanical properties test results of the AlCrTaN coatings prepared under different bias voltages show that the bias voltage affects the mechanical properties of the alloy. When -120 V, the coating has the highest hardness and the best fracture toughness. The elastic modulus gradually decreases with the increase of the bias voltage.
[0065] pass Figure 3 The friction coefficient test results of the AlCrTaN coatings prepared under different bias voltages show that at -100V, the friction coefficient of the coating is relatively high, exceeding 0.6, while the friction coefficients of the coatings prepared under the other three bias voltages are relatively low, between 0.5 and 0.6.
[0066] A preparation device for a tantalum-containing PVD hard coating, the preparation device comprising a base 1, on which a substrate surface treatment device 2, a glow cleaning device 3, an ion etching device 4 and an AlCrTaN coating deposition device 5 are installed, the substrate surface treatment device 2 comprising a box body, a support plate 20 is fixed in the box body, two electric push rods 15 are fixed in the box body, the output ends of the electric push rods 15 are fixedly connected to a clamping plate 16 that slides on the upper end of the support plate 20 for clamping the substrate, a hydraulic cylinder 6 is installed on the inner top of the box body, a movable plate 9 is fixed on the output end of the hydraulic cylinder 6, two sleeves 7 are fixed on the inner bottom of the box body, a sliding rod 8 is slidably connected in the sleeve 7, the lower end of the sliding rod 8 is fixedly connected to the upper end of the movable plate 9, so that the movable plate 9 can move up and down stably.
[0067] A change-over box 11 is fixedly connected to the bottom of the movable plate 9, and two bevel gears are meshed in the change-over box 11. Short rods are fixed to the axial ends of the two bevel gears, and the short rods penetrate the change-over box 11 and are rotatably connected thereto. A motor 10 is installed on the change-over box 11, and the output end of the motor 10 is fixedly connected to the short rod, and another short rod is fixedly connected to the polishing disk 12. A dust collecting box 18 is installed at the inner bottom of the box body, and a fan 19 is installed on the dust collecting box 18. The air inlet end of the fan 19 is connected to the dust collecting box 18, and a metal shaping hose 17 is fixed on the dust collecting box 18. A dust suction pipe 13 is installed on the metal shaping hose 17, and a plurality of dust suction holes 14 are penetrated through the dust suction pipe 13.
[0068] Put the YT15 hard alloy on the support plate 20, and the electric push rod 15 works to push the clamping plate 16 to move. The YT15 hard alloy can be clamped and fixed by the two clamping plates 16, and the hydraulic cylinder 6 is started. The hydraulic cylinder 6 drives the moving plate 9 to move downward. Under the guidance of the sleeve 7 and the sliding rod 8, the moving plate 9 moves stably, and then drives the motor 10 and the polishing plate 12 to move downward, so that the polishing plate 12 is against the upper end of the YT15 hard alloy. The motor 10 works to drive the polishing plate 12 to rotate, and the YT15 hard alloy can be polished by the polishing plate 12;
[0069] At the same time, the fan 19 is started. The fan 19 works to transport air to the dust box 18 through the dust suction hole 14, the dust suction pipe 13 and the metal shaping hose 17. The dust box 18 is installed with a filter located between the metal shaping hose 17 and the fan 19. The dust generated by the air during polishing enters the dust box 18, and the dust can be filtered and collected through the filter.
[0070] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A tantalum-containing PVD hard coating, comprising a substrate, characterized in that: The substrate is provided with a tantalum-containing PVD hard coating, which contains four elements: Al, Cr, Ta and N. The tantalum-containing PVD hard coating is an AlCrTaN coating, and the AlCrTaN coating has a nanostructure.
2. A tantalum-containing PVD hard coating according to claim 1, characterized in that: The AlCrTaN coating includes the following components in atomic percentage: 20-25% Cr, 5-10% Ta, 40-45% N, and the balance is Al.
3. A tantalum-containing PVD hard coating according to claim 1, characterized in that: The thickness of the AlCrTaN coating is in the range of 2 to 4 μm. The AlCrTaN coating consists of a Fcc-(Cr, Al)N phase. The Ta element in the AlCrTaN coating replaces Al or Cr to form a solid solution phase.
4. A tantalum-containing PVD hard coating according to claim 1, characterized in that: The hardness of the AlCrTaN coating is 30-35 GPa; the friction coefficient of the AlCrTaN coating is 0.5-0.6; the elastic modulus of the AlCrTaN coating is 400-530 GPa; and the bonding force of the AlCrTaN coating is 70-90N.
5. A method for preparing a novel tantalum-containing PVD hard coating according to any one of claims 1 to 4, characterized in that: Including the following processes: Process 1: surface pretreatment of the substrate; Process 2 is glow cleaning; Process three is ion etching treatment; Process four is the deposition of the AlCrTaN coating.
6. The method for preparing a tantalum-containing PVD hard coating according to claim 5, characterized in that: The surface pretreatment of the substrate includes first mechanically polishing the substrate, then ultrasonically cleaning the substrate in distilled water, acetone and alcohol in sequence, and drying the substrate for standby use.
7. The method for preparing a tantalum-containing PVD hard coating according to claim 5, characterized in that: The glow cleaning method is to fix the sample after surface pretreatment in a vacuum chamber and keep the pressure of the chamber at 10 -4 Pa, and then argon gas is introduced for glow discharge to remove impurities on the sample surface.
8. The method for preparing a tantalum-containing PVD hard coating according to claim 5, characterized in that: The ion etching process refers to using a pure Cr target to perform metal ion bombardment to remove surface impurities and increase the film-substrate bonding strength.
9. The method for preparing a tantalum-containing PVD hard coating according to claim 5, characterized in that: The deposition of the AlCrTaN coating includes two methods: The first method is arc deposition: AlCrTa alloy target is used as arc target, N2 is used as reaction gas, and AlCrTaN coating is deposited. The specific parameters are as follows: deposition temperature is 300-500℃, target current is 50-100A, nitrogen flow rate is 100-300sccm, gas pressure is 1-3Pa, deposition bias is -80V to -140V, deposition time is 30-200min, the distance between substrate and target is 10-15cm, and sample rotation and revolution are carried out simultaneously; The second method is magnetron + arc deposition: that is, AlCr alloy target is used as arc target and pure Ta target is used as magnetron target. In nitrogen atmosphere, magnetron sputtering Ta target and arc evaporation AlCr target are used to prepare AlCrTaN coating on the substrate surface. The specific parameters are as follows: deposition temperature is 300-500℃, nitrogen flow rate is 100-300sccm, gas pressure is 1-3Pa, deposition time is 30-200min, the distance between substrate and target is 10-15cm, arc target current is 50-100A, arc target deposition bias is -80V to -140V, and the average sputtering power of magnetron sputtering Ta target is 5-30W / cm 2 .
10. A preparation device for a tantalum-containing PVD hard coating, characterized in that: The preparation equipment comprises a base (1), on which a substrate surface treatment device (2), a glow cleaning device (3), an ion etching device (4) and an AlCrTaN coating deposition device (5) are installed, the substrate surface treatment device (2) comprises a box, a support plate (20) is fixed in the box, two electric push rods (15) are fixed in the box, the output end of the electric push rod (15) is fixedly connected to a clamping plate (16) sliding on the upper end of the support plate (20) for clamping the substrate, a hydraulic cylinder (6) is installed on the inner top of the box, a moving plate (9) is fixed on the output end of the hydraulic cylinder (6), and two sleeves (7) are fixed on the inner bottom of the box, a sliding rod (8) is slidably connected in the sleeve (7), and the lower end of the sliding rod (8) is fixedly connected to the upper end of the moving plate (9). The bottom of the movable plate (9) is fixedly connected to a direction-changing box (11), two bevel gears are meshed in the direction-changing box (11), short rods are fixed to the shaft ends of the two bevel gears, the short rods penetrate the direction-changing box (11) and are rotatably connected thereto, a motor (10) is installed on the direction-changing box (11), the output end of the motor (10) is fixedly connected to the short rods, and the other short rod is fixedly connected to a polishing disc (12), a dust collecting box (18) is installed on the inner bottom of the box body, a fan (19) is installed on the dust collecting box (18), the air inlet end of the fan (19) is connected to the dust collecting box (18), a metal shaping hose (17) is fixed on the dust collecting box (18), a dust suction pipe (13) is installed on the metal shaping hose (17), and a plurality of dust suction holes (14) are penetrated through the dust suction pipe (13).
Citation Information
Cited By
Tantalum-doped nitride coating and preparation method thereof
CN121380838A