Three-dimensional TiO2-Ag / AgCl composite material as well as preparation method and application thereof
By depositing TiO2 nanoneedles in situ on the surface of Ag foil and using the photosensitive nature of AgCl to generate active Ag to form a three-dimensional TiO2-Ag/AgCl composite material, the problems of complex and poor stability of the existing SERS substrate preparation process are solved, and high efficiency is achieved , stable molecular detection at very low concentrations.
Patent Information
- Application Number
- CN202411353987.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-09-27
AI Technical Summary
The existing SERS substrate preparation process is complex, costly and poorly stable, making it difficult to achieve efficient and stable extremely low concentration molecular detection, especially in applications in temperature, light and air environments.
Using three-dimensional TiO2-Ag/AgCl composite material, TiO2 nanoneedles were deposited in situ on the surface of Ag foil by hydrothermal reaction of titanium isopropoxide, concentrated hydrochloric acid and ethylene glycol. The photosensitive nature of AgCl was used to generate active Ag, and then through thermal migration. Form a stable three-dimensional structure to ensure the structural stability and SERS activity of the material.
It realizes simple and efficient material preparation, improves the structural stability and detection sensitivity of SERS substrates, can maintain efficient SERS activity for a long time in the indoor environment, and detects water pollutants such as extremely low concentrations of antibiotics.
Smart Images

Figure CN118883528A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of functional materials and Raman spectroscopy detection, and in particular to a three-dimensional TiO 2 -Ag / AgCl composite material and its preparation method and application. Background Art
[0002] Detecting extremely low concentrations of carcinogenic mutagens, early disease markers, antibiotics, various pesticide residues, industrial pollutants and other trace molecules from complex systems is an important topic in the field of modern analytical chemistry and biotechnology, and is also one of the key technologies to ensure food safety, public health and drug development. Raman spectroscopy is a fingerprint-like, inelastic scattering spectrum with molecular structure specificity. Surface-enhanced Raman technology (SERS), which has gradually developed based on Raman spectroscopy, does not require any external markers and can highly sensitively identify molecules by utilizing the special vibration characteristics of metal nanostructures. It has shown great potential and value in many fields such as materials science, biomedicine, and environmental monitoring. However, SERS technology still faces some challenges: (1) The heterogeneity of the analyte signal is uncontrollable; (2) The reproducibility of low-concentration analyte signals is not high. To address this problem, researchers have obtained a variety of complex SERS substrates or structures through various assembly techniques, such as substrate structures assembled from basic units such as zero-dimensional nanoparticles, one-dimensional nanowires, nanorods, two-dimensional nanosheets, nanodisks, nanoporous structures, and multi-level structures. The above structures all exhibit their unique Raman scattering properties, but this type of structure has many assembly steps, harsh preparation conditions, complex processes, high costs, low reuse rates, and is far from practical applications.
[0003] Developing simple, efficient and stable material preparation, processing and assembly methods is one of the important contents in developing efficient SERS substrates. 2 It is a semiconductor material with low price, bio-friendly, easy processing and great practical value. Its rich binding sites on the surface provide innate chemical advantages for material complexes and detection and identification of target molecules. Its relatively wide energy gap structure and adjustability provide convenience for matching the special energy levels of the molecules to be detected and satisfying the relevant charge transfer resonance. Precious metals (such as Au, Pt, etc.) can induce electric fields in SERS applications and significantly improve the detection limit of the molecules to be detected due to their unique local surface resonance (LSPR) effect. They are widely used as SERS active components or sites in many SERS substrates. However, in practical applications, it is usually necessary to consider the stability of precious metal nano-active units to temperature, light, acidity and alkalinity, and air to ensure that the entire SERS substrate has continuous detection activity and stability. Therefore, in order to improve the TiO 2In order to improve the performance of SERS substrate, in addition to improving the binding and electronic interactivity of the overall material structure to the molecules to be tested, it is also necessary to select suitable metal active ingredients so that the various components can be properly coupled to each other in a simple way, so as to ensure that the structure is stable and adjustable, and the SERS activity of the substrate can be maintained for a long time in indoor light and air environment.
[0004] The Chinese patent document with publication number CN105372223A discloses a Ag / TiO 2 Flexible, reusable SERS substrate and preparation method thereof, the invention uses thin Ti sheets as Ti source and prepares TiO based on Ti by hydrothermal synthesis method 2 Nanobelt arrays, Ag / TiO prepared by continuous ion deposition 2 SERS substrate material; Chinese patent document with publication number CN113670893A discloses a surface enhanced Raman scattering substrate and its preparation method and application. The method first uses a hydrothermal method to put a titanium foil into a reactor filled with a mixed solution of NaOH and urea to react, and prepares TiO2 with different morphologies by controlling the urea content. 2 Nanocone arrays; TiO 2 The nanocone array was plated with Ag to obtain Ag / TiO 2 The Ag / TiO 2 The substrate was used to detect SARS-CoV-2S1 protein. However, magnetron sputtering technology is expensive, the equipment is complex, and adverse phenomena such as gas discharge may occur, affecting the deposition quality. Summary of the invention
[0005] In order to solve the shortcomings of the prior art, the present invention provides a three-dimensional TiO 2 -Ag / AgCl composite material and its preparation method, which has good structural stability and adjustable structure, simple and efficient preparation method, relatively mild conditions, efficient and stable SERS activity, and can be used for high-sensitivity detection of water pollutants such as antibiotics.
[0006] The specific technical solutions adopted are as follows: A three-dimensional TiO 2 -A method for preparing an Ag / AgCl composite material, comprising the following steps: (1) Add titanium isopropoxide to a mixture of ethylene glycol, concentrated hydrochloric acid and water, stir, and then immerse the washed and dried Ag foil in the mixture. React at 80 to 150°C for 1.5 to 7.5 h to prepare Ag-based TiO substrate. 2 -AgCl; (2) Ag-based TiO 2- Place AgCl under a xenon lamp light source, control the light source current to irradiate the substrate, so that part of the AgCl components in the substrate undergo photoreduction to generate active single substance Ag; (3) Place the substrate after light treatment in a protective atmosphere and control the heating temperature to 200-500°C to allow the active element Ag to rely on TiO 2 The monomer undergoes thermal migration to prepare three-dimensional TiO 2 -Ag / AgCl composite material.
[0007] The present invention uses Ag foil as the base material, introduces an appropriate amount of concentrated hydrochloric acid, and simultaneously controls the chlorination rate of the Ag foil surface and the hydrolysis rate of titanium isopropoxide to make TiO 2 The in-situ deposition of nanostructured units and the in-situ evolution of AgCl crystals on the Ag foil surface work together to eventually "plant" a layer of disordered TiO on the Ag substrate. 2 Nano-needle-shaped "lawn"; AgCl crystal layer evolution and propagation rate is relatively fast, TiO 2 When the nanostructured monomers are deposited on the surface of the Ag foil, they are squeezed by the rapidly spreading AgCl crystal layer, which eventually causes the TiO 2 The monomers are firmly "planted" on the slits of the AgCl crystal layer, thus successfully assembling a layer of TiO on the Ag base. 2 Nano needle-like "lawn" structure; AgCl crystal layer is sensitive to light. Through light exposure, many active Ag(0) can be generated on its surface, and these active Ag(0) can rely on the nearby compatible TiO 2 The crystal plane migrates, so the TiO 2 The crystallinity of the nanostructures while controlling the TiO 2 Distribution of Ag(0) nanoparticles on the nanounit to prepare three-dimensional TiO 2 -Ag / AgCl composite material.
[0008] Optionally, the thickness of the Ag foil is 0.005-2.0 mm, the purity is 99.00%-99.998%, and the area is 0.5 cm×1.0 cm-4.0 cm×8.0 cm; the Ag foil is immersed in 0.01-0.5 mol / L HNO 3 The Ag foil was ultrasonically washed in the solution, isopropanol, acetone, ethanol, and deionized water for more than 30 min, taken out and blown dry with high-purity nitrogen to obtain the washed and dried Ag foil for use.
[0009] Preferably, in the mixed solution in step (1), the volume ratio of ethylene glycol, concentrated hydrochloric acid and water is 0.2-1:0.2-1:1; and the amount of titanium isopropoxide added is 1-5 v / v% based on the volume of water in the mixed solution.
[0010] Optionally, the substrate is Ag-based TiO 2 -AgCl was washed with isopropanol, acetone, ethanol and deionized water for multiple times and then put into use.
[0011] Specifically, in step (2), the wavelength of the xenon lamp light source is 300 nm ≤ λ ≤ 1100 nm, the xenon lamp light source exit window is 5.0 to 50 cm away from the substrate, and the light source current is controlled so that the irradiation intensity received by the substrate is 10.0 to 200 mW / cm 2 The irradiation time is controlled between 2.0 and 30 min. AgCl has photosensitivity. By controlling the light source current irradiation, the surface of the AgCl component in the substrate can be photoreduced to generate active Ag(0).
[0012] Optionally, in step (3), the protective atmosphere is a nitrogen atmosphere or a nitrogen-hydrogen mixed atmosphere, and the heating time is 30 to 120 min. 2 The three-dimensional structure of -AgCl is not destroyed in a protective atmosphere at ~500°C, and Ag(0) nanoparticles are formed from the substrate along the TiO 2 Nanoneedle thermal migration to prepare three-dimensional TiO with adjustable structure and properties 2 -Ag / AgCl composite material.
[0013] The present invention also provides the three-dimensional TiO 2 -Three-dimensional TiO prepared by the preparation method of Ag / AgCl composite material 2 -Ag / AgCl composite material.
[0014] The three-dimensional TiO 2 In-situ assembly of TiO on Ag foil substrate based on the mosaic effect of AgCl in Ag / AgCl composites 2 Nanoneedles, TiO 2 The nanoneedles form a lawn-like three-dimensional structure, TiO 2 Ag nanoparticles are randomly distributed on the nanoneedles; TiO 2 The length of the nanoneedle is 0.1 to 1 μm, the diameter is 10 to 60 nm, the particle size of the Ag nanoparticles is 5 to 40 nm, and the Ag nanoparticles are highly dispersed and not agglomerated.
[0015] The present invention also provides the three-dimensional TiO 2 -Application of Ag / AgCl composite materials in surface enhanced Raman scattering detection.
[0016] The present invention also provides a method for detecting antibiotics in an aqueous solution, using the three-dimensional TiO 2 -Ag / AgCl composite material. Specifically, the three-dimensional TiO2 -Ag / AgCl composite material is in contact with the aqueous solution to be tested, and Raman spectroscopy is performed after drying.
[0017] Optionally, the antibiotic is a quinolone antibiotic such as norfloxacin, norfloxacin, ofloxacin, ciprofloxacin, and fleroxacin.
[0018] Experiments have shown that the use of the three-dimensional TiO 2 -Ag / AgCl composite materials can stably detect concentrations below 10 - 6 mol / L norfloxacin solution, the detection limit can reach 10 -10 mol / L, and the three-dimensional TiO 2 -Ag / AgCl composites have long-lasting SERS activity.
[0019] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention provides a three-dimensional TiO 2 -Ag / AgCl composite material in situ preparation method, by using Ag foil as the source material of the substrate, through the in situ hydrothermal reaction with titanium isopropoxide, hydrochloric acid and ethylene glycol, TiO 2 The nanostructure units are assembled onto the Ag foil surface synchronously with the help of the chlorination process on the Ag foil surface. The AgCl component in the composite structure acts as a photosensitizer and provides an active Ag(0) migration source for the composite structure after photoreduction. After heat treatment in an inert gas or 5% reducing atmosphere, a three-dimensional TiO 2 -Ag / AgCl composite material, the three-dimensional TiO 2 In-situ assembly of TiO on Ag foil substrate based on the mosaic effect of AgCl in Ag / AgCl composites 2 Nanoneedles, TiO 2 The nanoneedles form a lawn-like three-dimensional structure, TiO 2 Ag nanoparticles are randomly distributed on the nanoneedles.
[0020] (2) The continuous in-situ assembly and processing method of the present invention expands the composite form between materials with mismatched lattices and expands the application scope of materials; the functional material components of the structure are more randomly and uniformly distributed, and the nanostructure is conducive to the increase of specific surface area; TiO 2 The nanoneedle units are squeezed by the AgCl crystal layer on the substrate surface, so that each TiO 2 The nanoneedle "lawn" structure can be firmly "planted" on the Ag substrate and has structural stability; the three-dimensional TiO 2-The heterogeneous interface and SERS performance of the Ag / AgCl composite material structure are highly stable and can maintain SERS activity for a long time in indoor light, temperature and air environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The three-dimensional TiO prepared in Example 1 2 -SEM image of Ag / AgCl composite material, scale bar 40 μm.
[0022] Figure 2 The three-dimensional TiO prepared in Example 1 2 -SEM image of Ag / AgCl composite material, scale bar 100 nm.
[0023] Figure 3 The three-dimensional TiO prepared in Example 1 2 -Process XRD patterns of Ag / AgCl composites.
[0024] Figure 4 The three-dimensional TiO prepared in Example 2 2 -SEM image of Ag / AgCl composite material, scale bar 100 μm.
[0025] Figure 5 The three-dimensional TiO prepared in Example 2 2 -SEM image of Ag / AgCl composite material, scale bar 200 nm.
[0026] Figure 6 The three-dimensional TiO prepared in Example 2 2 -Process XRD patterns of Ag / AgCl composites.
[0027] Figure 7 The three-dimensional TiO prepared in Example 3 2 -SEM image of Ag / AgCl composite material, scale bar 15 μm.
[0028] Figure 8 The three-dimensional TiO prepared in Example 3 2 -SEM image of Ag / AgCl composite material, scale bar 2 μm.
[0029] Fig. 9 The three-dimensional TiO prepared in Example 3 2 -Process XRD patterns of Ag / AgCl composites.
[0030] Fig.10 The three-dimensional TiO prepared in Example 1 2 -Ag / AgCl composite material for 10 -4 ~10 -10SERS detection spectrum of mol / L norfloxacin solution.
[0031] Fig.11 The three-dimensional TiO prepared in Example 1 2 -Ag / AgCl composite material for 10 consecutive days -6 mol / L norfloxacin solution SERS detection stability comparison chart. DETAILED DESCRIPTION
[0032] The present invention will be further described below in conjunction with the examples and drawings. It should be understood that these examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. The operating methods in the following examples that do not specify specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer. Contents not described in detail in this specification belong to prior art known to professionals and technicians in the field.
[0033] In the embodiment, the flat Ag foil used has a thickness of 0.005-2.0 mm and a purity of 99.00%-99.998%. It is cut into foils with an area of 0.5 cm×1.0 cm-4.0 cm×8.0 cm and immersed in 0.1-1 mol / L HNO 3 The solution was ultrasonically washed in isopropanol, acetone, ethanol, and deionized water for more than 30 min, and then taken out and dried with high-purity nitrogen for later use.
[0034] Example 1 Step 1: In-situ assembly of Ag-based TiO substrate 2 -AgCl; Add 2 ml of concentrated hydrochloric acid to 10 ml of deionized water and stir thoroughly; then add 4 ml of ethylene glycol and mix thoroughly to obtain a mixed solution; slowly add titanium isopropoxide dropwise to a volume of 0.2 ml and stir thoroughly to mix thoroughly; immerse the cleaned and dried Ag foil that has been ultrasonically washed in dilute nitric acid, isopropanol, acetone, ethanol, and deionized water in the above solution, seal it, and then perform a hydrothermal reaction at 120°C, and control the reaction time to 2.5 h to prepare the substrate Ag-based TiO 2 -AgCl, and the substrate was washed with isopropanol, acetone, ethanol, and deionized water for multiple times for standby use.
[0035] Step 2: Photoinduced generation of active elemental Ag on the AgCl surface; The prepared substrate Ag-based TiO 2 -AgCl was placed horizontally under a xenon lamp light source (300nm ≤ λ ≤ 1100 nm), with the light source exit window 30 cm away from the substrate sample. The light control mode of the light source was used to control the light source current so that the irradiation intensity received by the substrate sample was 100 mW / cm2 The irradiation time was 5 min. The photosensitivity of AgCl was utilized to photoreduced the surface of the AgCl component in the composite structure to generate active single substance Ag. The obtained sample was stored dry at room temperature for later use.
[0036] Step 3: Active elemental Ag forms Ag particles distributed on TiO through thermal migration 2 On the structural monomer; The Ag-based TiO 2 The AgCl composite structure was placed in a tube furnace in a nitrogen atmosphere and heated at 300°C for 60 min to make the active Ag on the surface of AgCl rely on TiO 2 Nanomonomers undergo thermal migration in TiO 2 Ag nanoparticles are randomly distributed in batches on the monomer, and finally a three-dimensional TiO 2 -Ag / AgCl composite material, the three-dimensional TiO 2 -SEM images of Ag / AgCl composites Figure 1 and Figure 2 As shown, TiO 2 The length of the nanoneedle is about 200-300 nm, the diameter is between 20-50 nm, the particle size of the Ag nanoparticle is about 5-20 nm, and the three-dimensional TiO 2 -XRD characterization of Ag / AgCl composites Figure 3 As shown in the figure, the diffraction spectrum shows rutile TiO 2 , typical diffraction peaks of cubic AgCl and Ag crystals, with no other impurity phase signals.
[0037] Example 2 The difference between this embodiment and embodiment 1 is that in step 1, the addition of 10 ml of deionized water is changed to 7 ml of deionized water, and the addition of 4 ml of ethylene glycol can be changed to 7 ml of ethylene glycol. The other parameters and processes are the same as those in embodiment 1. The three-dimensional TiO 2 -Ag / AgCl composite materials, in which TiO 2 The aspect ratio of the monomer structure is different from that of Example 1; the three-dimensional TiO 2 -SEM images of Ag / AgCl composites Figure 4 and Figure 5 As shown, TiO 2 The length of the nanoneedle is about 0.8-1 μm, the diameter is about 50-60 nm, the particle size of the Ag nanoparticle is about 10-30 nm, and the XRD characterization of the process is as follows: Figure 6 As shown in the figure, the diffraction spectrum shows rutile TiO 2, typical diffraction peaks of cubic AgCl and Ag crystals, with no other impurity phase signals.
[0038] Example 3 The difference between this embodiment and embodiment 1 is that in step 1, the addition of 2 ml of concentrated hydrochloric acid is changed to 7 ml of concentrated hydrochloric acid, and the addition of 10 ml of deionized water is changed to 7 ml of deionized water. Other parameters and processes are the same as those in embodiment 1, and three-dimensional TiO 2 -Ag / AgCl composite materials, in which TiO 2 The nanoneedles are composed of micron-sized balls filling the gaps in the AgCl block. 2 -SEM images of Ag / AgCl composites Figure 7 and Figure 8 As shown, TiO 2 The length of the nanoneedle is about 0.4-0.8 μm, the diameter is about 5-20 nm, and the particle size of the Ag nanoparticles is about 5-40 nm. The process XRD pattern is shown in Fig. 9 As shown in the figure, the diffraction spectrum shows rutile TiO 2 , typical diffraction peaks of cubic AgCl and Ag crystals, with no other impurity phase signals.
[0039] Sample analysis The three-dimensional TiO prepared in Example 1 was tested 2 -SERS activity and stability of Ag / AgCl composites in indoor light, temperature and air environment; The concentrations used were 10 -4 mol / L、10 -6 mol / L、10 -8 mol / L、10 -10 mol / L norfloxacin antibiotic solution was used as the test object; the three-dimensional TiO 2 -Ag / AgCl composite material was cut into 4 pieces and randomly numbered 1 to 4; 10 -4 mol / L、10 -6 mol / L、10 -8 mol / L、10 -10 mol / L norfloxacin solution, the volume of the solution added was 5 μL, and after natural drying under the same conditions, Raman spectroscopy was performed. The laser wavelength used in the test was 633 nm, the number of integrations was 3, and 20 points of each sample were randomly tested 20 times. The surface enhancement spectrum obtained after averaging is shown in the figure below. Fig.10 As shown. Fig.10 It can be seen that when the three-dimensional TiO 2 -Ag / AgCl composite material was used to detect norfloxacin solution.-4 ~10 -10 mol / L norfloxacin solution has a high SERS detection activity. 2 -Ag / AgCl composite material was cut into 10 pieces, randomly numbered 1 to 10, and stored in a glass container at room temperature, air atmosphere, and 50% humidity. One sample substrate was taken every day according to the number and compared with the newly configured 10 -6 The same Raman test was performed on mol / L norfloxacin solution. The laser wavelength used for the test was 633 nm, the number of integrations was 3, and 20 points of each sample were randomly tested 20 times. The average surface enhancement spectrum was as follows: Fig.11 As shown, the three-dimensional TiO 2 -Ag / AgCl composite material has a certain long-term effect on the SERS activity of norfloxacin solution. 2 -Ag / AgCl composite materials are used in the detection and identification of agricultural residues in water, food additives, environmental analysis, drug analysis, biochemistry, etc.
[0040] The embodiments described above provide a detailed description of the technical solutions of the present invention. It should be understood that the above are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, supplements or similar substitutions made within the scope of the principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a three-dimensional TiO2-Ag / AgCl composite material, characterized in that: The following steps are involved: (1) adding titanium isopropoxide to a mixture of ethylene glycol, concentrated hydrochloric acid and water, stirring, and then immersing the washed and dried Ag foil therein, reacting at a heating environment of 80 to 150° C. for 1.5 to 7.5 h to prepare a substrate Ag-based TiO2-AgCl; (2) placing the Ag-based TiO2-AgCl substrate under a xenon lamp light source, controlling the light source current to irradiate the substrate, so that part of the AgCl component in the substrate undergoes photoreduction to generate active elemental Ag; (3) Placing the light-treated substrate in a protective atmosphere, controlling the heating temperature at 200-500°C, allowing the active single substance Ag to thermally migrate with the TiO2 monomer to prepare a three-dimensional TiO2-Ag / AgCl composite material.
2. The method for preparing the three-dimensional TiO2-Ag / AgCl composite material according to claim 1, characterized in that: The thickness of Ag foil is 0.005 to 2.0 mm, and the purity is 99.00% to 99.998%.
3. The method for preparing the three-dimensional TiO2-Ag / AgCl composite material according to claim 1, characterized in that: In the mixed solution in step (1), the volume ratio of ethylene glycol, concentrated hydrochloric acid and water is 0.2-1:0.2-1:1; and the amount of titanium isopropoxide added is 1-5 v / v% based on the volume of water in the mixed solution.
4. The method for preparing the three-dimensional TiO2-Ag / AgCl composite material according to claim 1, characterized in that: In step (2), the wavelength of the xenon lamp light source is 300 nm ≤ λ ≤ 1100 nm, the xenon lamp light source exit window is 5.0 to 50 cm away from the substrate, and the light source current is controlled so that the irradiation intensity received by the substrate is 10.0 to 200 mW / cm 2 The irradiation time was controlled between 2.0 and 30 min.
5. The method for preparing the three-dimensional TiO2-Ag / AgCl composite material according to claim 1, characterized in that: In step (3), the protective atmosphere is a nitrogen atmosphere or a nitrogen-hydrogen mixed atmosphere, and the heating time is 30 to 120 min.
6. A three-dimensional TiO2-Ag / AgCl composite material obtained according to the method for preparing a three-dimensional TiO2-Ag / AgCl composite material according to any one of claims 1 to 5.
7. The three-dimensional TiO2-Ag / AgCl composite material according to claim 6, characterized in that: In the three-dimensional TiO2-Ag / AgCl composite material, TiO2 nanoneedles are in-situ assembled on an Ag foil substrate based on the inlay effect of AgCl, the TiO2 nanoneedles form a lawn-like three-dimensional structure, and Ag nanoparticles are randomly distributed on the TiO2 nanoneedles; the length of the TiO2 nanoneedles is 0.2 to 1 μm, the diameter is 10 to 60 nm, and the particle size of the Ag nanoparticles is 5 to 40 nm.
8. Use of the three-dimensional TiO2-Ag / AgCl composite material according to claim 6 or 7 in surface enhanced Raman scattering detection.
9. A method for detecting antibiotics in an aqueous solution, characterized in that: Use the three-dimensional TiO2-Ag / AgCl composite material according to claim 6 or 7.
10. The method for detecting antibiotics in an aqueous solution according to claim 9, characterized in that: The antibiotics are quinolone antibiotics, including norfloxacin, ofloxacin, ciprofloxacin or fleroxacin.
Citation Information
Patent Citations
Ag / AgCl / TiO2 compound photocatalytic material and preparation method and application thereof
CN107456983A
Preparation method for raman spectrum detection substrate
CN108896530A
Preparing method and application of photoinduced enhanced Raman substrate based on TiO2 / Ag nanoarray
CN109112601A
Preparation method of nano composite photocatalyst AgCl / ZIF-8 and nano composite photocatalyst prepared thereby
CN111545246A
Precious metal modified titanium dioxide nanorod array with excellent surface enhanced Raman scattering property and preparation method and application of precious metal modified titanium dioxide nanorod array