Method and system for preparing carbon-encapsulated silicon nanoparticles
Carbon nanoparticles are generated through plasma generators and mixed with silicon nanoparticles in the high-temperature reaction chamber to form carbon-encapsulated silicon nanoparticles, solving the stability and life problems of existing silicon carbon anode materials in the charge and discharge cycle, realizing the The effect of better quality materials and reducing production costs.
Patent Information
- Application Number
- CN202411353990.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-27
AI Technical Summary
The existing silicon carbon negative electrode materials have problems such as material crushing, active substances falling off and battery pack deformation during the charge and discharge cycle, which affects the cycle stability and life of the battery.
Carbon nanoparticles are generated through a plasma generator, and the silicon nanoparticles and carbon nanoparticles are mixed in a high-temperature reaction chamber to form carbon-encapsulated silicon nanoparticles. This method uses plasma technology to directly prepare carbon nanoparticles, and achieves uniform encapsulation of silicon nanoparticles through the reaction chamber.
The preparation of better silicon carbon negative electrode materials is achieved, which improves the circulation stability and battery life of the materials and reduces production costs.
Smart Images

Figure CN118888736B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of silicon-carbon negative electrode material preparation, and in particular to a method and system for preparing carbon-wrapped silicon nanoparticles. Background Art
[0002] Silicon negative electrode is a choice with a theoretical specific capacity far higher than that of graphite negative electrode, and its related application research has been developing; new energy vehicle companies have been gradually using silicon materials as negative electrode battery packs.
[0003] Most of the current silicon negative electrodes are silicon-carbon negative electrodes. This is because the volume of silicon materials can expand by up to 300% during the charge and discharge process, which can cause problems such as material breakage, active material shedding, and battery pack deformation in a charge and discharge cycle, which seriously affects the cycle stability and life of the battery. Therefore, the current mainstream idea is to use silicon-carbon negative electrodes, that is, to wrap nano-silicon particles in carbon particles.
[0004] Based on this, how to prepare silicon-carbon negative electrode materials has become a hot research direction. The main methods for preparing silicon-carbon negative electrodes currently include: using porous carbon coating, that is, injecting silicon nanoparticles into porous carbon particles through a jet, but in the process of injecting silicon nanoparticles into porous carbon, some silicon nanoparticles will adhere to the surface of the porous carbon, that is, not all silicon nanoparticles can be encapsulated in the porous carbon particles. The silicon-carbon negative electrode materials prepared by this scheme still have certain charge and discharge cycle instability problems.
[0005] In order to obtain higher quality silicon-carbon negative electrode materials and avoid the problems existing in the above methods, the present invention proposes a new method and system for preparing carbon-encapsulated silicon nanoparticles. Summary of the invention
[0006] The object of the present invention is to provide a method and system for preparing carbon-encapsulated silicon nanoparticles, which adopts a method different from the prior art silicon-carbon negative electrode material preparation method process to produce a higher quality silicon-carbon negative electrode material.
[0007] The present invention is achieved through the following technical solutions:
[0008] In a first aspect, a method for preparing carbon-encapsulated silicon nanoparticles is provided, comprising:
[0009] A carbon source gas is introduced into a plasma generator as a working gas to generate carbon nanoparticles by cracking.
[0010] Passing silicon nanoparticles and carbon nanoparticles into a reaction chamber with a high temperature environment;
[0011] Silicon nanoparticles and carbon nanoparticles are mixed in the reaction chamber and flow from the feed inlet to the discharge outlet to form carbon-wrapped silicon nanoparticles.
[0012] Furthermore, the silicon nanoparticles are obtained as follows:
[0013] The silicon powder is vaporized by a plasma generator to generate the silicon nanoparticles;
[0014] The temperature of the plasma flame emitted by the plasma generator is higher than 2300°C.
[0015] Furthermore, the temperature maintenance method in the reaction chamber is as follows:
[0016] A plasma flame is injected between the inlet and outlet of the reaction chamber to maintain the ambient temperature required for the combination of silicon nanoparticles and carbon nanoparticles in the reaction chamber.
[0017] Furthermore, the step of introducing the silicon nanoparticles and the carbon nanoparticles into a reaction chamber having a high temperature environment is specifically as follows:
[0018] The silicon nanoparticles and carbon nanoparticles enter the reaction chamber through different feed inlets.
[0019] Furthermore, before the silicon nanoparticles are introduced into the reaction chamber, they are electrochemically charged with positive or negative charges; before the carbon nanoparticles are introduced into the reaction chamber, they are electrochemically charged with charges opposite to those of the silicon nanoparticles.
[0020] In the second aspect, based on the above principle method, a method for preparing carbon-encapsulated silicon nanoparticles which is easier to be applied in practice is provided, comprising:
[0021] Silicon nanoparticles generated by vaporizing silicon powder through a first plasma generator are introduced into a reaction chamber through a first feed inlet; an interface of a third plasma generator is provided between the feed inlet and the discharge port of the reaction chamber, and a plasma flame is injected into the reaction chamber through the third plasma generator to maintain a target ambient temperature in the reaction chamber;
[0022] A carbon source gas is introduced into the second plasma generator as a working gas to generate carbon nanoparticles by cracking, and the carbon nanoparticles are introduced into the reaction chamber through the second feed inlet;
[0023] A negative pressure is generated at the discharge port of the reaction chamber by means of a vacuum device, so that the silicon nanoparticles and the carbon nanoparticles flow from the inlet of the reaction chamber to the discharge port, forming carbon-wrapped silicon nanoparticles.
[0024] Furthermore, before the silicon nanoparticles are introduced into the reaction chamber through the first feed port, the process further comprises:
[0025] The silicon nanoparticles are made to pass through the first high-voltage electrostatic chamber at high speed, so that the silicon nanoparticles are positively charged or negatively charged.
[0026] Furthermore, before the carbon nanoparticles are introduced into the reaction chamber through the second feed port, the process further comprises:
[0027] The carbon nanoparticles are made to pass through the second high-voltage electrostatic chamber at high speed, so that the carbon nanoparticles have charges opposite to those of the silicon nanoparticles.
[0028] Furthermore, the number of the third plasma generators is positively correlated with the distance between the feed inlet and the discharge outlet.
[0029] Furthermore, the temperature of the plasma flame generated by the first plasma generator is 2600-3000°C; the temperature of the plasma flame generated by the second plasma generator is 800-1500°C; the temperature of the plasma flame generated by the third plasma generator is 800-850°C, and the working gas is an inert gas.
[0030] In a third aspect, based on the implementation of the above specific method, a system for preparing carbon-encapsulated silicon nanoparticles is provided, comprising:
[0031] A reaction chamber, the reaction chamber comprising a first feed inlet, a second feed inlet, a discharge port and a flange interface; the first feed inlet and the second feed inlet are both located at a first end of the reaction chamber, the discharge port is located at a second end away from the first end, and the flange interface is arranged between the first end and the second end; the discharge port is also connected to a negative pressure generating device;
[0032] A silicon nanoparticle generating device, comprising a first plasma generator, a powder feeder and a powder making chamber; a powder outlet of the powder feeder and a flame outlet of the first plasma generator are both arranged in the powder making chamber, the powder making chamber comprises a silicon nanoparticle outlet, and the silicon nanoparticle outlet is connected to a first feed inlet;
[0033] A carbon nanoparticle generating device, the carbon nanoparticle generating device comprising a second plasma generator and a cracking chamber; the flame outlet of the second plasma generator is arranged in the cracking chamber, the cracking chamber comprises a carbon nanoparticle outlet, and the carbon nanoparticle outlet is connected to a second feed inlet;
[0034] A third plasma generator is arranged on the reaction chamber through the flange interface.
[0035] Furthermore, a first high-voltage electrostatic chamber is provided between the silicon nanoparticle outlet and the first feed inlet; a first gas acceleration section is also provided between the silicon nanoparticle outlet and the first high-voltage electrostatic chamber, and the first gas acceleration section is used to allow the gas flow carrying silicon nanoparticles to pass through the first high-voltage electrostatic chamber at a first preset speed;
[0036] A second high-voltage electrostatic chamber is also arranged between the carbon nanoparticle outlet and the second feed inlet; a second gas acceleration section is also included between the carbon nanoparticle outlet and the second high-voltage electrostatic chamber, and the second gas acceleration section is used to allow the gas flow carrying carbon nanoparticles to pass through the second high-voltage electrostatic chamber at a second preset speed.
[0037] The technical solution of the present invention has at least the following advantages and beneficial effects:
[0038] The present invention provides a novel method for producing carbon-encapsulated silicon nanoparticles which is easy to realize industrially. The method uses a plasma generator to crack a carbon source gas as a working gas to produce carbon nanoparticles. The carbon nanoparticles and silicon nanoparticles are passed through a reaction chamber in a high-temperature environment to combine the particles of the two, thereby forming carbon-encapsulated silicon nanoparticles. The method of the present invention directly obtains carbon nanoparticles based on plasma technology treatment, and combines the carbon-encapsulated silicon nanoparticles through the reaction chamber. The process does not involve the storage of the carbon nanoparticle raw materials, which is beneficial to reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 A schematic diagram of a method flow chart provided in Example 1 of the present invention;
[0040] Figure 2 A schematic diagram of a method flow chart provided in Example 2 of the present invention;
[0041] Figure 3 A schematic diagram of the system structure provided in Example 3 of the present invention;
[0042] Figure 4 This is an electron microscope image of carbon-encapsulated silicon nanoparticles prepared by the technical solution of the present invention;
[0043] Figure 5 This is an electron microscope image of the edge of carbon-encapsulated silicon nanoparticles prepared by the technical solution of the present invention. DETAILED DESCRIPTION
[0044] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.
[0045] Currently, the use of silicon-carbon negative electrode materials is one of the mainstream ways to improve battery performance, and there are some related technical solutions for preparing silicon-carbon negative electrode materials. A current mainstream and easy-to-implement method is to use porous carbon coating, that is, to drive silicon nanoparticles into porous carbon particles by jet or other methods. However, in the process of driving silicon nanoparticles into porous carbon, some silicon nanoparticles will adhere to the surface of the porous carbon, that is, not all silicon nanoparticles can be wrapped in porous carbon particles, and silicon nanoparticles attached to the surface of porous carbon will still have a certain impact on the battery. Based on this, the present invention proposes a new method for preparing carbon-coated silicon nanoparticles.
[0046] Example 1
[0047] This embodiment provides a method for preparing carbon-encapsulated silicon nanoparticles. Figure 1 As shown, the principle of the method is as follows: by mixing the prepared silicon nanoparticles and carbon nanoparticles in a reaction place with a high temperature environment (800-850°C), after a certain period of time, the silicon nanoparticles are wrapped by the carbon nanoparticles to form carbon-wrapped silicon nanoparticles. It should be noted that the particle size of the silicon nanoparticles is larger than that of the carbon nanoparticles, such as Figure 4 It is knowable.
[0048] Specifically in the present invention, considering the need for easy industrial production, we use carbon source gas as working gas to pass into the plasma generator (i.e., the second plasma generator), the reaction temperature is about 800-1500°C, and the carbon nanoparticles are cracked; wherein the carbon source gas includes methane, carbon dioxide, etc. In the present invention, methane is preferred, and less additional products are produced during its cracking process.
[0049] Silicon nanoparticles and carbon nanoparticles are introduced into a reaction chamber with a high temperature environment; the silicon nanoparticles and carbon nanoparticles are mixed in the reaction chamber and flow from the feed port to the discharge port to form carbon-encapsulated silicon nanoparticles. In this scheme, the prepared silicon nanoparticles can be directly sent into the reaction chamber to combine with the carbon nanoparticles produced by the cracking of the plasma generator to form carbon-encapsulated silicon nanoparticles. It should be noted that the silicon nanoparticles and carbon nanoparticles enter the reaction chamber through different feed ports; that is, the silicon nanoparticles and carbon nanoparticles are processed through independent channels in the early stage.
[0050] Since the preservation requirements of silicon nanoparticles are relatively strict, in industrial production, if ready-made silicon nanoparticles are directly used, a good preservation environment is required, such as storing nano-scale silicon particles in an inert gas to prevent agglomeration and oxidation, which will increase the cost of industrial implementation. In comparison, the preservation of silicon micron-scale particles is easier to achieve and the cost is relatively low.
[0051] Therefore, in order to reduce the cost of industrial production, the present invention proposes a preferred embodiment, that is, using silicon micron-sized particles to directly prepare silicon nanoparticles at the production site; the specific method is as follows:
[0052] Silicon powder (micron level) is vaporized by a plasma generator to produce silicon nanoparticles; it should be noted that here the silicon nanoparticles are mainly prepared by plasma technology, and in the actual implementation process, the preparation equipment can refer to the powder preparation system and related working methods recorded in the Chinese invention patent CN117339520A, a non-metallic ultrafine powder preparation system and method based on plasma transferred arc. The plasma flame temperature emitted by the plasma generator (i.e., the first plasma generator) in this part of the equipment system needs to be 2600-3000℃.
[0053] For the reaction chamber, the place where the silicon nanoparticles and carbon nanoparticles are combined inside it needs to maintain a relatively high ambient temperature; conventionally, a wrapping heating method can be used to maintain the temperature inside the reaction chamber, such as wrapping the entire reaction chamber in a heating chamber heated by an electric heating wire. This method is easy to implement, but the control of the temperature inside the reaction chamber is relatively slow, because the heat follows the heat transfer path from the air to the reaction chamber structure and then to the air inside the reaction chamber. Therefore, this method is not sensitive to temperature control, and once the device is shut down, it takes a long time to restart.
[0054] Therefore, in the embodiment of the present invention, a flange interface penetrating the reaction chamber wall is provided in the reaction chamber, and a plasma generator (i.e., a third plasma generator) is connected through the flange interface. The plasma generator directly heats the reaction chamber to a required temperature of 800-850°C.
[0055] In order to make the silicon nanoparticles and carbon nanoparticles fully combined in the reaction chamber, the reaction chamber can be extended in the length direction. In order to maintain the required temperature in the longer reaction chamber, multiple flange interfaces for fixing the plasma generator can be evenly spaced on the reaction chamber. Regarding the matching relationship between the length of the reaction chamber and the number of plasma generators, according to the current experimental practice data, it is better to configure a plasma generator every 0.5-1m interval of the reaction chamber to maintain the temperature stability inside the reaction chamber.
[0056] The reaction time of silicon nanoparticles and carbon nanoparticles in the reaction chamber is affected by two factors: the length of the reaction chamber and the exhaust speed of the negative pressure generating device at one end of the reaction chamber outlet. Since the data such as the size of the reaction chamber have been solidified in advance during the industrial manufacturing process, the main influencing factor in the actual preparation process is the exhaust speed of the negative pressure generating device at one end of the reaction chamber outlet; the reaction and combination time of silicon nanoparticles and carbon nanoparticles in the reaction chamber is controlled by controlling the exhaust speed of the negative pressure generating device.
[0057] In order to make the silicon nanoparticles and the carbon nanoparticles combine quickly in the reaction chamber, this embodiment also proposes a method, that is, before the silicon nanoparticles are introduced into the reaction chamber, they are charged with positive or negative charges by an electrochemical method; and before the carbon nanoparticles are introduced into the reaction chamber, they are charged with charges opposite to those of the silicon nanoparticles by an electrochemical method. Since the silicon nanoparticles and the carbon nanoparticles enter the reaction chamber through different channels, a high-voltage electrostatic chamber (i.e., a first high-voltage electrostatic chamber and a second high-voltage electrostatic chamber) can be added to the channel near the reaction chamber, and the silicon nanoparticles and the carbon nanoparticles are charged with charges of opposite polarities by the high-voltage electrostatic chamber, so that the two can be quickly combined when entering the reaction chamber.
[0058] The carbon-encapsulated silicon nanoparticles prepared by the technical solution of the present invention have good expected effects. Figure 4 , Figure 5 As shown, it is an electron microscope image of a sample made by the manufacturing method of the present application, and it can be seen that the carbon nanoparticles completely encapsulate the silicon nanoparticles. Figure 4 The dark-colored part in the center is silicon nanoparticles, and the light-colored part wrapped around it is carbon nanoparticles. Figure 5 The edge contact between silicon nanoparticles and carbon nanoparticles shows good contact. From the electron microscope images above, it can be seen that the prepared carbon-wrapped silicon nanoparticles meet the requirements for application in battery manufacturing.
[0059] Also from Figure 4 It can be seen that the silicon nanoparticles are much larger than the carbon nanoparticles; in order to allow the silicon nanoparticles to be quickly wrapped with a layer of carbon nanoparticles, when charging the silicon nanoparticles and the carbon nanoparticles, the charge carried by the silicon nanoparticles needs to be much larger than the charge carried by the carbon nanoparticles and with opposite electrical polarity.
[0060] Example 2
[0061] This embodiment provides a method for preparing carbon-encapsulated silicon nanoparticles that is easier to apply in practice based on the principle of Embodiment 1. Figure 2 As shown, the details are as follows:
[0062] Silicon nanoparticles generated by vaporizing silicon powder through a first plasma generator are introduced into a reaction chamber through a first feed inlet; an interface of a third plasma generator is provided between the feed inlet and the discharge port of the reaction chamber, and a plasma flame is injected into the reaction chamber through the third plasma generator to maintain a target ambient temperature in the reaction chamber;
[0063] A carbon source gas is introduced into the second plasma generator as a working gas to generate carbon nanoparticles by cracking, and the carbon nanoparticles are introduced into the reaction chamber through the second feed inlet;
[0064] A negative pressure is generated at the discharge port of the reaction chamber by means of a vacuum device, so that the silicon nanoparticles and the carbon nanoparticles flow from the inlet of the reaction chamber to the discharge port, forming carbon-wrapped silicon nanoparticles.
[0065] As mentioned in Example 1, in order to accelerate the combination of the two particles, before the silicon nanoparticles are introduced into the reaction chamber through the first feed port, the silicon nanoparticles are passed through the first high-voltage electrostatic chamber at high speed, thereby making the silicon nanoparticles have positive or negative charges.
[0066] Before the carbon nanoparticles are introduced into the reaction chamber through the second feed port, the carbon nanoparticles are passed through the second high-voltage electrostatic chamber at high speed, so that the carbon nanoparticles have an opposite charge to the silicon nanoparticles. Since the two have opposite charges, they can be quickly combined after entering the reaction chamber.
[0067] In the embodiment of the present invention, a flange interface penetrating the reaction chamber wall is provided in the reaction chamber, and a third plasma generator is connected through the flange interface. The reaction chamber is directly heated by the third plasma generator to reach a required temperature.
[0068] In order to fully combine the silicon nanoparticles and the carbon nanoparticles in the reaction chamber, the reaction chamber can be extended in the length direction. In order to maintain the required temperature in the longer reaction chamber, multiple flange interfaces for fixing the third plasma generator can be evenly spaced on the reaction chamber. It can be seen that the number of the third plasma generator is positively correlated with the distance between the feed port and the discharge port.
[0069] For the above scheme, the temperature requirements of the plasma flames of various types of plasma generators in this embodiment are as follows: the temperature of the plasma flame generated by the first plasma generator is 2600-3000°C; the temperature of the plasma flame generated by the second plasma generator is 800-1500°C; the temperature of the plasma flame generated by the third plasma generator is 800-850°C, and the working gas adopts inert gas.
[0070] Example 3
[0071] This embodiment provides a specific system design solution based on the principles of Embodiments 1 and 2. Figure 3 As shown, it should be noted that Figure 3 The arrows in the figure indicate the flow direction of gas and particles. It is particularly noted that the third plasma generator uses inert gas as the working gas, and the high-temperature plasma flame it generates directly acts on the inside of the reaction chamber. Therefore, the arrows point to the high-temperature gas into the reaction chamber, which specifically includes:
[0072] The reaction chamber comprises a first feed inlet, a second feed inlet, a discharge port and a flange interface; the first feed inlet and the second feed inlet are both located at the first end of the reaction chamber, the discharge port is located at the second end away from the first end, and the flange interface is arranged between the first end and the second end; the discharge port is also connected to a negative pressure generating device.
[0073] Silicon nanoparticle production equipment, the silicon nanoparticle production equipment includes a first plasma generator, a powder feeder and a powder making chamber; the powder outlet of the powder feeder and the flame outlet of the first plasma generator are both arranged in the powder making chamber, the powder making chamber includes a silicon nanoparticle outlet, and the silicon nanoparticle outlet is connected to the first feed inlet. The equipment can refer to the powder preparation system and related working methods recorded in the Chinese invention patent CN117339520A, a non-metallic ultrafine powder preparation system and method based on plasma transferred arc.
[0074] The carbon nanoparticle generating device comprises a second plasma generator and a cracking chamber; the flame outlet of the second plasma generator is arranged in the cracking chamber, the cracking chamber comprises a carbon nanoparticle outlet, and the carbon nanoparticle outlet is connected to the second feed port.
[0075] The third plasma generator is arranged on the reaction chamber through a flange interface.
[0076] In order to make the silicon nanoparticles and carbon nanoparticles combine quickly in the reaction chamber, a first high-voltage electrostatic chamber is also provided between the silicon nanoparticle outlet and the first feed inlet; a first gas acceleration section is also provided between the silicon nanoparticle outlet and the first high-voltage electrostatic chamber, and the first gas acceleration section is used to make the gas flow with silicon nanoparticles pass through the first high-voltage electrostatic chamber at a first preset speed. A second high-voltage electrostatic chamber is also provided between the carbon nanoparticle outlet and the second feed inlet; a second gas acceleration section is also provided between the carbon nanoparticle outlet and the second high-voltage electrostatic chamber, and the second gas acceleration section is used to make the gas flow with carbon nanoparticles pass through the second high-voltage electrostatic chamber at a second preset speed.
[0077] Since the electrochemical method is adopted, the high-voltage electrostatic chamber is a cavity that only includes the particle delivery and output ports, and the cavity is equipped with electrodes; the electrodes should include a positive electrode (grounded or connected to a high-voltage power supply) and a negative electrode (grounded or connected to a high-voltage power supply); that is, in one high-voltage electrostatic chamber, the positive electrode is grounded and the negative electrode is connected to the high-voltage power supply; in another high-voltage electrostatic chamber, the positive electrode is connected to the high-voltage power supply and the negative electrode is grounded; the electrode spacing is moderate to ensure that the particles can pass quickly but can obtain sufficient charge; the electrode shape can be flat or mesh to improve the uniformity of the electric field. In order to prevent the electrode from adsorbing the particles, a first gas acceleration section is also included between the silicon nanoparticle outlet and the first high-voltage electrostatic chamber, and a second gas acceleration section is also included between the carbon nanoparticle outlet and the second high-voltage electrostatic chamber; the acceleration section accelerates the airflow carrying the particles, so that the particles pass through the high-voltage electrostatic chamber through the high-speed airflow, and then when they are charged, they are not adsorbed by the electrodes, so that the particles can smoothly enter the subsequent reaction chamber.
[0078] The gas acceleration section can be to reduce the diameter of the gas outlet port, thereby increasing the gas pressure at the gas outlet end to achieve the purpose of increasing the gas flow rate, or it can be an external high-speed airflow device that directly introduces high-speed airflow into the corresponding pipeline. It should be noted that when using external equipment to introduce high-speed airflow into the pipeline, inert gas should be used. Figure 3 The solution in the invention is to use external equipment to introduce high-speed airflow into the pipeline.
[0079] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing carbon-encapsulated silicon nanoparticles, characterized in that: include: A carbon source gas is introduced into a plasma generator as a working gas to generate carbon nanoparticles by cracking. Passing silicon nanoparticles and carbon nanoparticles into a reaction chamber with a high temperature environment; Silicon nanoparticles and carbon nanoparticles are mixed in the reaction chamber and flow from the feed inlet to the discharge outlet to form carbon-wrapped silicon nanoparticles.
2. The method for preparing carbon-encapsulated silicon nanoparticles according to claim 1, characterized in that: The silicon nanoparticles are obtained as follows: The silicon powder is vaporized by a plasma generator to generate the silicon nanoparticles; The temperature of the plasma flame emitted by the plasma generator is higher than 2300°C.
3. The method for preparing carbon-encapsulated silicon nanoparticles according to claim 1, characterized in that: The temperature maintenance method in the reaction chamber is as follows: A plasma flame is injected between the inlet and outlet of the reaction chamber to maintain the ambient temperature in the reaction chamber required for the silicon nanoparticles and the carbon nanoparticles to combine.
4. The method for preparing carbon-encapsulated silicon nanoparticles according to any one of claims 1 to 3, characterized in that: The step of introducing the silicon nanoparticles and the carbon nanoparticles into a reaction chamber having a high temperature environment is specifically as follows: The silicon nanoparticles and carbon nanoparticles enter the reaction chamber through different feed inlets.
5. The method for preparing carbon-encapsulated silicon nanoparticles according to claim 4, characterized in that: Before the silicon nanoparticles are introduced into the reaction chamber, they are charged with positive or negative charges by electrochemical methods; before the carbon nanoparticles are introduced into the reaction chamber, they are charged with charges opposite to those of the silicon nanoparticles by electrochemical methods.
6. A method for preparing carbon-encapsulated silicon nanoparticles, characterized in that: include: Silicon nanoparticles generated by vaporizing silicon powder through a first plasma generator are introduced into a reaction chamber through a first feed inlet; an interface of a third plasma generator is provided between the feed inlet and the discharge port of the reaction chamber, and a plasma flame is injected into the reaction chamber through the third plasma generator to maintain a target ambient temperature in the reaction chamber; A carbon source gas is introduced into the second plasma generator as a working gas to generate carbon nanoparticles by cracking, and the carbon nanoparticles are introduced into the reaction chamber through a second feed inlet; A negative pressure is generated at the discharge port of the reaction chamber by means of a vacuum device, so that the silicon nanoparticles and the carbon nanoparticles flow from the inlet of the reaction chamber to the discharge port, forming carbon-wrapped silicon nanoparticles.
7. The method for preparing carbon-encapsulated silicon nanoparticles according to claim 6, characterized in that: Before the silicon nanoparticles are introduced into the reaction chamber through the first feed port, the method further comprises: The silicon nanoparticles are made to pass through the first high-voltage electrostatic chamber at high speed, so that the silicon nanoparticles are positively charged or negatively charged.
8. The method for preparing carbon-encapsulated silicon nanoparticles according to claim 7, characterized in that: Before the carbon nanoparticles are introduced into the reaction chamber through the second feed port, the method further comprises: The carbon nanoparticles are made to pass through the second high-voltage electrostatic chamber at high speed, so that the carbon nanoparticles have charges opposite to those of the silicon nanoparticles.
9. The method for preparing carbon-encapsulated silicon nanoparticles according to claim 6, characterized in that: The number of the third plasma generators is positively correlated with the distance between the feed inlet and the discharge outlet.
10. The method for preparing carbon-encapsulated silicon nanoparticles according to any one of claims 6 to 9, characterized in that: The temperature of the plasma flame generated by the first plasma generator is 2600-3000°C; the temperature of the plasma flame generated by the second plasma generator is 800-1500°C; the temperature of the plasma flame generated by the third plasma generator is 800-850°C, and the working gas is an inert gas.
11. A system for preparing carbon-encapsulated silicon nanoparticles, characterized in that: include: A reaction chamber, the reaction chamber comprising a first feed inlet, a second feed inlet, a discharge port and a flange interface; the first feed inlet and the second feed inlet are both located at a first end of the reaction chamber, the discharge port is located at a second end away from the first end, and the flange interface is arranged between the first end and the second end; the discharge port is also connected to a negative pressure generating device; A silicon nanoparticle generating device, comprising a first plasma generator, a powder feeder and a powder making chamber; a powder outlet of the powder feeder and a flame outlet of the first plasma generator are both arranged in the powder making chamber, the powder making chamber comprises a silicon nanoparticle outlet, and the silicon nanoparticle outlet is connected to a first feed inlet; A carbon nanoparticle generating device, the carbon nanoparticle generating device comprising a second plasma generator and a cracking chamber; the flame outlet of the second plasma generator is arranged in the cracking chamber, the cracking chamber comprises a carbon nanoparticle outlet, and the carbon nanoparticle outlet is connected to a second feed inlet; A third plasma generator is arranged on the reaction chamber through the flange interface.
12. The system for preparing carbon-encapsulated silicon nanoparticles according to claim 11, characterized in that: A first high-voltage electrostatic chamber is also provided between the silicon nanoparticle outlet and the first feed inlet; a first gas acceleration section is also provided between the silicon nanoparticle outlet and the first high-voltage electrostatic chamber, and the first gas acceleration section is used to allow the gas flow carrying silicon nanoparticles to pass through the first high-voltage electrostatic chamber at a first preset speed; A second high-voltage electrostatic chamber is also arranged between the carbon nanoparticle outlet and the second feed inlet; a second gas acceleration section is also included between the carbon nanoparticle outlet and the second high-voltage electrostatic chamber, and the second gas acceleration section is used to allow the gas flow carrying carbon nanoparticles to pass through the second high-voltage electrostatic chamber at a second preset speed.
Citation Information
Patent Citations
Non-metal ultrafine powder preparation system and method based on plasma transferred arc
CN117339520A
Silicon-carbon cathode material and method for preparing same
CN106898755A
Method for preparing high-performance silicon-carbon negative electrode composite material of lithium ion battery
CN109742372A
Ultrafine carbon material dual-mode plasma reaction device and preparation method thereof
CN111908445A
Production method of carbon-coated nano silicon powder used as negative electrode material of lithium ion battery