DAC adsorbent and preparation process thereof

Through the preparation of nano-scale metal alumina powder and aerogel composite materials, the problems of low adsorption capacity and high regeneration energy consumption in DAC technology are solved, and efficient and stable CO2 adsorption performance and low environmental pollution are achieved.

CN118892813AInactive Publication Date: 2024-11-05HEIJING ENERGY DEV CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411131162.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-17
Publication Date
2024-11-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing DAC technology is difficult to effectively capture and treat carbon dioxide in the atmosphere due to the problems of low adsorption capacity, slow adsorption rate, poor cycle stability and high regeneration energy consumption.

Method used

Using nano-scale metal alumina powder and aerogel composite materials, the preparation process includes mixing of sodium alginate, kappa carrageenan and chitosan, carbonization treatment, ultrasonic oscillation and magnetic stirring, etc., to prepare excellent pore structures. and nano-scale metal alumina adsorbents with large specific surface area.

Benefits of technology

It significantly improves the CO2 adsorption performance and stability of the adsorbent, reduces the use of chemical reagents and environmental pollution during the preparation process, and achieves efficient adsorption performance under a wider range of environmental conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892813A_ABST
    Figure CN118892813A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of carbon dioxide adsorption, and particularly discloses a DAC adsorbent and a preparation process thereof. Sodium alginate, kappa-type carrageenan and chitosan are evenly mixed according to the mass ratio of 3: 1: 2 to serve as a precursor material of aerogel, and then the precursor material is prepared into a precursor aqueous solution with the mass fraction of 3%; preliminary forming and drying of aerogel: using ethanol as a coagulating bath, separating out gel through a wet spinning technology, placing the separated gel fiber in a Cu (NO3) 2 solution with the mass fraction of 5% for further coagulation forming, drying the formed gel at 60 DEG C, and removing residual moisture; the adsorbent has an excellent pore structure and a relatively large specific surface area, so that rich active sites are provided for subsequent metal ion loading, and the adsorption performance of the adsorbent is remarkably enhanced, so that the adsorbent can keep stable adsorption performance under wider environmental conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of carbon dioxide adsorption, and in particular relates to a DAC adsorbent and a preparation process thereof. Background Art

[0002] With the acceleration of global industrialization and population growth, environmental pollution problems are becoming increasingly serious, especially the rising concentration of carbon dioxide (CO2) in the air, which has led to global warming and frequent extreme weather events, posing a serious threat to human living environment and economic development. According to statistics from the International Energy Agency, the annual global CO2 emissions have reached billions of tons and are showing an increasing trend year by year. Therefore, the development of efficient CO2 capture technology is of great significance for mitigating climate change;

[0003] Direct Air Capture (DAC) technology is an emerging CO2 emission reduction technology that captures CO2 directly from the atmosphere by adsorption or absorption, and has the potential to become one of the key technologies for achieving negative emission targets in the future. However, DAC technology still faces many challenges in practical applications, such as low adsorption capacity of adsorbents, slow adsorption rate, poor cycle stability, and high regeneration energy consumption.

[0004] Traditional DAC adsorbents mainly include alkali metal hydroxides, amine-based adsorbent materials, molecular sieves, activated carbon, etc. Although these materials can achieve CO2 capture to a certain extent, their performance is often limited by various factors. For example, although alkali metal hydroxides have a high CO2 adsorption capacity, their regeneration process consumes a lot of energy and there are serious equipment corrosion problems; although amine-based adsorbent materials have a faster adsorption rate, their regeneration temperature is high and performance degradation is prone to occur under long-term use; although materials such as molecular sieves and activated carbon have a large specific surface area, their selective adsorption capacity for CO2 is limited;

[0005] Therefore, developing a new DAC adsorbent with high adsorption capacity, fast adsorption kinetics, good cycle stability and low regeneration energy consumption has become a hot topic in current research. In this context, the present invention proposes a new DAC adsorbent and its preparation process. Summary of the invention

[0006] The object of the present invention is to provide a DAC adsorbent and a preparation process thereof to solve the problems raised in the above background technology.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] DAC adsorbent preparation process, including:

[0009] S1. preparing nano-scale metal aluminum oxide powder;

[0010] S2. preparing an aerogel precursor: mixing sodium alginate, κ-type carrageenan and chitosan in a mass ratio of 3:1:2 to obtain an aerogel precursor material, and then preparing the mixture into a precursor aqueous solution with a mass fraction of 3%;

[0011] S3. Preliminary forming and drying of aerogel: using ethanol as a coagulation bath, the gel is precipitated by wet spinning technology, the precipitated gel fiber is placed in a 5% by mass Cu(NO3)2 solution for further coagulation, and the formed gel is dried at 60°C to remove residual moisture;

[0012] S4, preparing aerogel: placing the dried gel in a muffle furnace and carbonizing it at 800° C. for 2 hours, soaking the carbonized aerogel in a weak acid, then washing it with deionized water to remove impurities, and drying the washed aerogel under dry conditions for later use;

[0013] S5. Preparation of composite adsorption material: Asp was dissolved in 10 mL of 6.0 mol / L NaOH solution, and 0.3 g of aerogel was added, and ultrasonic oscillation was performed for 30 minutes to uniformly disperse the aerogel in the solution to obtain a mixed solution, 100 mL of 0.5 mol / L Cu(NO3)2 solution was slowly added dropwise to the uniformly dispersed mixed solution, and the mixture was reacted for 3 hours under magnetic stirring. After the reaction was completed, a solid product was obtained by centrifugal separation;

[0014] S6, washing and drying: washing with deionized water, weak acid and water + ethanol (volume ratio 1:1) for multiple times, drying at 100° C. for 24 hours to obtain a composite adsorption material;

[0015] S7. Preparation of adsorbent: dissolve the composite adsorbent material in methanol or deionized water to obtain a mixed solution, add the prepared nano-scale metal alumina powder into the mixed solution and stir, then evaporate the excess liquid through a rotary evaporator, place the sample in a vacuum drying oven for vacuum drying, and obtain a nano-scale metal alumina adsorbent.

[0016] Preferably, in S1, the method for preparing the nano-scale metal aluminum oxide powder is specifically:

[0017] S11, solution preparation: prepare an aqueous solution containing 1 mmol / L of aluminum salt, prepare an aqueous solution of Na2CO3 with a concentration of 0.5 mmol / L, the volume of which is the same as that of the aqueous solution of aluminum salt, and prepare an aqueous solution of NaOH with a concentration of 1 mmol / L to 10 mmol / L;

[0018] S12, pH adjustment: slowly add dilute hydrochloric acid to the Na2CO3 aqueous solution while monitoring the pH value until it reaches and is maintained in the range of 9 to 11;

[0019] S13, mixing and pH maintenance: under normal temperature and continuous stirring, adding aluminum salt aqueous solution to the Na2CO3 aqueous solution at a uniform speed and slowly, and at the same time, dropping NaOH aqueous solution into the Na2CO3 aqueous solution to maintain the pH value of the solution in the range of 9 to 11, and continuing for 30 minutes to 90 minutes;

[0020] S14, aging treatment: aging the mixed solution at room temperature with continuous stirring for 16 to 24 hours;

[0021] S15, washing and neutralization: the aged solution is fully washed with deionized water by centrifugation or filtration until it reaches neutrality. During this process, ensure that the sample is always kept moist;

[0022] S16, organic solvent washing: washing the sample after deionized water washing with an organic solvent, also keeping the sample in a wet state;

[0023] S17, organic solvent dispersion and maintenance: disperse the sample after washing with the organic solvent into the same organic solvent solution, maintain this state for 4 to 6 hours at room temperature and under continuous stirring, and wash the sample again with the same organic solvent used previously;

[0024] S18, vacuum drying: vacuum drying the washed samples at 60°C to 70°C for not less than 12 hours;

[0025] S19, calcination treatment: place the dried sample in a N2 protected atmosphere furnace, and calcine it at a temperature of 400° C. to 500° C. for 4 h to 6 h to obtain nano-scale metal aluminum oxide powder.

[0026] Preferably, the organic solvent is one of ethanol or acetone.

[0027] A DAC adsorbent prepared according to any of the above preparation methods.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] It has an excellent pore structure and a large specific surface area, which provides abundant active sites for subsequent metal ion loading, significantly enhances the adsorption performance of the adsorbent, and enables the adsorbent to maintain stable adsorption performance under a wider range of environmental conditions. Relatively few chemical reagents are used in the entire preparation process, and most of the reagents can be recycled or safely disposed of, reducing pollution to the environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Embodiment 1:

[0033] See also Figure 1 As shown, the DAC adsorbent preparation process comprises:

[0034] S1. preparing nano-scale metal aluminum oxide powder;

[0035] S2. preparing an aerogel precursor: mixing sodium alginate, κ-type carrageenan and chitosan in a mass ratio of 3:1:2 to obtain an aerogel precursor material, and then preparing the mixture into a precursor aqueous solution with a mass fraction of 3%;

[0036] S3. Preliminary forming and drying of aerogel: using ethanol as a coagulation bath, the gel is precipitated by wet spinning technology, the precipitated gel fiber is placed in a 5% by mass Cu(NO3)2 solution for further coagulation, and the formed gel is dried at 60°C to remove residual moisture;

[0037] S4, preparing aerogel: placing the dried gel in a muffle furnace and carbonizing it at 800° C. for 2 hours, soaking the carbonized aerogel in a weak acid, then washing it with deionized water to remove impurities, and drying the washed aerogel under dry conditions for later use;

[0038] S5. Preparation of composite adsorption material: Asp was dissolved in 10 mL of 6.0 mol / L NaOH solution, and 0.3 g of aerogel was added, and ultrasonic oscillation was performed for 30 minutes to uniformly disperse the aerogel in the solution to obtain a mixed solution, 100 mL of 0.5 mol / L Cu(NO3)2 solution was slowly added dropwise to the uniformly dispersed mixed solution, and the mixture was reacted for 3 hours under magnetic stirring. After the reaction was completed, a solid product was obtained by centrifugal separation;

[0039] S6, washing and drying: washing with deionized water, weak acid and water + ethanol (volume ratio 1:1) for multiple times, drying at 100° C. for 24 hours to obtain a composite adsorption material;

[0040] S7. Preparation of adsorbent: dissolve the composite adsorbent material in methanol or deionized water to obtain a mixed solution, add the prepared nano-scale metal alumina powder into the mixed solution and stir, then evaporate the excess liquid through a rotary evaporator, place the sample in a vacuum drying oven for vacuum drying, and obtain a nano-scale metal alumina adsorbent.

[0041] In one embodiment of the present invention, in S1, the method for preparing nano-scale metal aluminum oxide powder is specifically:

[0042] S11, solution preparation: prepare an aqueous solution containing 1 mmol / L of aluminum salt, prepare an aqueous solution of Na2CO3 with a concentration of 0.5 mmol / L, the volume of which is the same as that of the aqueous solution of aluminum salt, and prepare an aqueous solution of NaOH with a concentration of 1 mmol / L to 10 mmol / L;

[0043] S12, pH adjustment: slowly add dilute hydrochloric acid to the Na2CO3 aqueous solution while monitoring the pH value until it reaches and is maintained in the range of 9 to 11;

[0044] S13, mixing and pH maintenance: under normal temperature and continuous stirring, adding aluminum salt aqueous solution to the Na2CO3 aqueous solution at a uniform speed and slowly, and at the same time, dropping NaOH aqueous solution into the Na2CO3 aqueous solution to maintain the pH value of the solution in the range of 9 to 11, and continuing for 30 minutes to 90 minutes;

[0045] S14, aging treatment: aging the mixed solution at room temperature with continuous stirring for 16 to 24 hours;

[0046] S15, washing and neutralization: the aged solution is fully washed with deionized water by centrifugation or filtration until it reaches neutrality. During this process, ensure that the sample is always kept moist;

[0047] S16, organic solvent washing: washing the sample after deionized water washing with an organic solvent, also keeping the sample in a wet state;

[0048] S17, organic solvent dispersion and maintenance: disperse the sample after washing with the organic solvent into the same organic solvent solution, maintain this state for 4 to 6 hours at room temperature and under continuous stirring, and wash the sample again with the same organic solvent used previously;

[0049] S18, vacuum drying: vacuum drying the washed samples at 60°C to 70°C for not less than 12 hours;

[0050] S19. Calcination treatment: Place the dried sample in a N2 protected atmosphere furnace and calcine it at a temperature of 400° C. to 500° C. for 4 to 6 hours to obtain nano-scale metal aluminum oxide powder.

[0051] In one embodiment of the present invention, the organic solvent is one of ethanol or acetone.

[0052] A DAC adsorbent prepared according to any of the above preparation methods.

[0053] Experimental example:

[0054] The fixed bed cycle adsorption method was used to conduct the CO2 adsorption experiment. 1.0g of dry adsorbent was placed in a fixed bed adsorption column with an inner diameter of 10mm. The fixed bed was connected to the gas circulation system, and the gas flow rate was adjusted to 300mL / min for the adsorption experiment. The environment was set to 298K and 0.1MPa. The comparison of CO2 adsorption capacity of the adsorbent is shown in the following table:

[0055] Composite adsorbent Temperature / K <![CDATA[CO2 adsorption capacity / (mg·g -1 )]]> <![CDATA[UiO-66-(OH)2 / GO]]> 298 191 MOF / GO-U3 277 320 CG-9 273 363 Cu-BTC / GO10 298 243 MOF / GO-U3 303 186 Nano-scale metal alumina adsorbent 298 323

[0056] From the above, it can be seen that the composite adsorbent retains the dual advantages of the skeleton material's high CO2 adsorption capacity and the aerogel's rapid adsorption, and therefore has a higher CO2 adsorption potential.

[0057] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. DAC adsorbent preparation process, It is characterized in that include: S1. preparing nano-scale metal aluminum oxide powder; S2. preparing an aerogel precursor: mixing sodium alginate, κ-type carrageenan and chitosan in a mass ratio of 3:1:2 to obtain an aerogel precursor material, and then preparing the mixture into a precursor aqueous solution with a mass fraction of 3%; S3. Preliminary forming and drying of aerogel: Using ethanol as a coagulation bath, the gel was precipitated by wet spinning technology, and the precipitated gel fiber was placed in a 5% by mass Cu(NO 3 ) 2 The solution is further solidified and formed, and the formed gel is dried at 60°C to remove residual moisture; S4, preparing aerogel: placing the dried gel in a muffle furnace and carbonizing it at 800° C. for 2 hours, soaking the carbonized aerogel in a weak acid, then washing it with deionized water to remove impurities, and drying the washed aerogel under dry conditions for later use; S5. Preparation of composite adsorption material: Asp was dissolved in 10 mL of 6.0 mol / L NaOH solution, and 0.3 g of aerogel was added. Ultrasonic oscillation was performed for 30 minutes to disperse the aerogel evenly in the solution to obtain a mixed solution. 100 mL of 0.5 mol / L Cu(NO 3 ) 2 The solution was slowly added dropwise to the uniformly dispersed mixed solution, and reacted for 3 hours under magnetic stirring. After the reaction was completed, a solid product was obtained by centrifugal separation; S6, washing and drying: washing with deionized water, weak acid and water + ethanol (volume ratio 1:1) for multiple times, drying at 100° C. for 24 hours to obtain a composite adsorption material; S7. Preparation of adsorbent: dissolve the composite adsorbent material in methanol or deionized water to obtain a mixed solution, add the prepared nano-scale metal alumina powder into the mixed solution and stir, then evaporate the excess liquid through a rotary evaporator, place the sample in a vacuum drying oven for vacuum drying, and obtain a nano-scale metal alumina adsorbent.

2. The DAC adsorbent and its preparation process according to claim 1, Features: In S1, the preparation method of nano-scale metal aluminum oxide powder is specifically: S11, solution preparation: prepare an aqueous solution containing 1mmol / L aluminum salt, prepare a sodium 2 CO 3 Aqueous solution, the volume of which is the same as that of the aluminum salt aqueous solution, is prepared with a concentration of 1 mmol / L to 10 mmol / L of NaOH aqueous solution; S12, pH adjustment: to Na 2 CO 3 Slowly add dilute hydrochloric acid to the aqueous solution while monitoring the pH value until it reaches and is maintained in the range of 9 to 11; S13, Mixing and pH maintenance: At room temperature and under continuous stirring, add Na 2 CO 3 Aluminum salt solution was added to the aqueous solution at a uniform speed and slowly. 2 CO 3 NaOH aqueous solution is added dropwise into the aqueous solution to maintain the pH value of the solution in the range of 9 to 11 for 30 to 90 minutes; S14, aging treatment: aging the mixed solution at room temperature with continuous stirring for 16 to 24 hours; S15, washing and neutralization: the aged solution is fully washed with deionized water by centrifugation or filtration until it reaches neutrality. During this process, ensure that the sample is always kept moist; S16, organic solvent washing: washing the sample after deionized water washing with an organic solvent, also keeping the sample in a wet state; S17, organic solvent dispersion and maintenance: disperse the sample after washing with the organic solvent into the same organic solvent solution, maintain this state for 4 to 6 hours at room temperature and under continuous stirring, and wash the sample again with the same organic solvent used previously; S18, vacuum drying: vacuum drying the washed samples at 60°C to 70°C for not less than 12 hours; S19, calcination treatment: the dried sample is placed in N 2 The nano-sized metal aluminum oxide powder is calcined in a protective atmosphere furnace at a temperature of 400° C. to 500° C. for a duration of 4 to 6 hours.

3. The DAC adsorbent and its preparation process according to claim 2, Features: The organic solvent is one of ethanol or acetone.

4. The DAC adsorbent prepared according to any one of the preparation methods of claims 1-2.

Citation Information

Patent Citations

  • A preparing method of a nanofluid reinforcing gas-liquid mass transfer of a CO2 absorbent and applications of the nanofluid

    CN104607023A

  • Preparation method of block metal catalyst with attapulgite-alumina aerogel as carrier

    CN113198547A

  • DAC adsorbent and preparation method thereof

    CN116371382A

  • Method for integrating carbon dioxide trapping and hydrogenation methanol preparation by using Cu-based catalyst

    CN118059905A

  • Carbon dioxide adsorption material convenient to dissociate and regenerate

    CN118179433A