Sodium alginate-polyamidoxime composite hydrogel sphere uranium adsorption material and preparation method thereof

Through the preparation and cross-linking process of sodium alginate-polyaminoxime composite hydrogel ball material, the problems of insufficient stability and poor selectivity of existing adsorbent materials are solved, and efficient uranium ion adsorption and selectivity are achieved, which is suitable for Extraction of marine uranium resources.

CN118892816AInactive Publication Date: 2024-11-05HARBIN ENG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410958461.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-07-10
Filing Date
2024-07-17
Publication Date
2024-11-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing materials used to adsorb uranium have problems such as insufficient stability, low adsorption capacity and poor selectivity.

Method used

The composite gel liquid is prepared by mechanical stirring and cross-linking, and cross-linking is performed using calcium ions and glutaraldehyde to form a rich amino group and ligand. Microporous spherical adsorption material of amidoxime functional groups.

Benefits of technology

It has achieved efficient adsorption of uranium ions, with high adsorption rate and selectivity, especially at pH 6, the uranium ion removal rate can reach more than 95%, and it still maintains good selectivity in the presence of multiple coexisting ions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892816A_ABST
    Figure CN118892816A_ABST
Patent Text Reader

Abstract

The invention discloses a sodium alginate-polyamidoxime composite hydrogel sphere uranium adsorbent and a preparation method thereof, and relates to a uranium adsorption material and a preparation method thereof. The invention aims to solve the problems of insufficient stability, low adsorption capacity and poor selectivity of the existing adsorption material with amidoxime group for extracting uranium. Sodium alginate and hyperbranched polyamide molecules are adopted as the basis, after sodium alginate is subjected to calcium ion forming, a gel structure is reinforced through covalent cross-linking to enhance the stability, a three-dimensional gel network is formed through cross-linking of a hyperbranched structure, polyamidoxime is introduced into the gel network, and through two-time forming of ionic cross-linking and covalent cross-linking, the stability of the hydrogel is improved. The sodium alginate-poly (amidoxime / amide) composite gel ball with a three-dimensional porous structure is constructed. The hydrogel ball adsorption material contains rich amidoxime functional groups, shows excellent adsorption capacity and ion selectivity to uranium, and has excellent mechanical strength. The method is suitable for preparing the hydrogel sphere uranium adsorbent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a sodium alginate-polyamidoxime composite hydrogel spherical uranium adsorption material and a preparation method thereof. Background Art

[0002] Developing clean energy to replace fossil fuels is an effective way, among which nuclear energy has attracted widespread attention as a recognized clean energy. Uranium is the main component of nuclear fuel in nuclear energy. Currently, uranium mainly comes from terrestrial mineral resources. However, with the development of nuclear energy, the uranium reserves on land have shown a shortage trend and are expected to be exhausted in the next 80-120 years. At the same time, the ocean contains rich uranium resources. It is estimated that there are 4.5 billion tons of uranium in the ocean, which is 1,000 times the uranium reserves on land, and can provide energy supply for the nuclear industry for thousands of years. The main form of uranium in the ocean is uranyl ions. However, since the concentration of uranium in seawater is very low and there are many interfering ions, exploring a selective, efficient and economical extraction method is a necessary condition for obtaining uranium resources in the ocean.

[0003] Existing methods for extracting uranium mainly include membrane separation, ion exchange, solvent absorption, adsorption, etc. Among them, the adsorption method has become an effective and economical method due to its simple process, low cost, high efficiency and environmental friendliness, and is widely used. The key to the adsorption method is to design efficient and economical adsorption materials.

[0004] Hydrogel materials have attracted much attention due to their unique solid-liquid dual properties and good morphology controllability. Among them, sodium alginate (SA)-based gel ball materials not only have the universal properties of hydrogels, but also their granular macroscopic morphology is more suitable for a variety of adsorption devices and easy to directly recycle. At the same time, the preparation scheme of sodium alginate (SA)-based gel ball materials is simple, the raw materials are cheap and easy to obtain, and they have good benefits in the opening of adsorption materials. Although SA-based gel balls can be used to remove uranium ions from aqueous solutions, adsorption based on carboxyl groups alone cannot obtain good uranium selectivity. Polyamidoximes (PAOs) have excellent performance in uranium recovery in solution due to their wide range of amidoxime functional groups with strong complexing ability and selectivity. However, due to the strong intermolecular hydrogen bonds, the molecular chains are easy to agglomerate and the hydrophilicity is reduced, which leads to problems such as insufficient stability and adsorption capacity, which limits its direct application. Summary of the invention

[0005] The purpose of the present invention is to solve the problems of insufficient stability, low adsorption capacity and poor selectivity of existing materials for adsorbing uranium. A sodium alginate-polyamidoxime composite hydrogel spherical uranium adsorption material and a preparation method thereof are proposed.

[0006] The structural formula of the sodium alginate-polyamidoxime composite hydrogel spherical uranium adsorption material of the present invention is:

[0007]

[0008] The preparation method of the sodium alginate-polyamidoxime composite hydrogel spherical uranium adsorption material of the present invention is carried out according to the following steps:

[0009] 1. Preparation of composite gel solution using polyamidoxime, sodium alginate and hyperbranched polyamide as raw materials:

[0010] Weighing sodium alginate powder and dissolving it in deionized water to obtain a sodium alginate solution; weighing polyamidoxime powder and dissolving it in a sodium hydroxide solution to obtain an alkaline polyamidoxime solution; weighing hyperbranched polyamide powder and dissolving it in deionized water to obtain a polyamide solution; adding the polyamidoxime solution and the polyamide solution to the sodium alginate solution and mechanically stirring them at room temperature, and then standing to obtain a composite gel solution;

[0011] The ratio of the mass of the sodium alginate powder to the volume of deionized water is (400-700) mg: (8-20) mL;

[0012] The ratio of the mass of the polyamidoxime powder to the volume of the sodium hydroxide solution is (0.15-1) g: (8-20) mL;

[0013] The concentration of the sodium hydroxide solution is 0.4-0.7 mol / L;

[0014] The ratio of the mass of the hyperbranched polyamide powder to the volume of deionized water is (0.25-2) g: (4.5-8) mL;

[0015] The mass ratio of sodium alginate to polyamidoxime is 1:(0.5-1.5); the mass ratio of polyamidoxime to hyperbranched polyamide is 1:(1.2-2.5);

[0016] The mechanical stirring time is 10-40 minutes, and the standing time is 15-40 minutes;

[0017] 2. Cross-linking the composite gel solution obtained in step 1 twice to obtain sodium alginate-polyamidoximine composite hydrogel spheres;

[0018] The process of the double cross-linking is as follows: dropping the composite gel solution obtained in step 1 into a calcium ion solution for primary cross-linking molding, then filtering and washing with deionized water for several times to obtain gel balls; then placing the gel balls in a glutaraldehyde solution for secondary cross-linking molding, shaking during the secondary cross-linking molding process, then washing the gel balls with deionized water for several times, and finally freeze-drying to obtain a sodium alginate-polyamidooxime composite hydrogel ball uranium adsorption material;

[0019] The time of the primary cross-linking molding is 1-5 hours, and the calcium ion solution is a calcium chloride solution with a concentration of 2-4wt.%;

[0020] The secondary cross-linking molding time is 7-12 hours, and the mass fraction of the glutaraldehyde solution is 1.5-4%.

[0021] The principles and beneficial effects of the present invention are:

[0022] 1. The sodium alginate-polyamidoxime composite hydrogel sphere uranium adsorption material of the present invention contains abundant amino and amidoxime functional groups, exhibits excellent adsorption capacity for uranium, has high adsorption rate and uranium ion selectivity; has the highest adsorption capacity at pH 6, and has a high adsorption rate at concentration C 0 =100ppm, pH=6 uranium solution, the removal rate of uranium ions can reach more than 95% (the adsorption amount can reach more than 475mg / g).

[0023] 2. Due to the synergistic adsorption effect of amino and amidoxime groups, additional binding sites are provided and affinity is enhanced during the coordination process with uranium ions, thereby improving the adsorption efficiency and capacity of uranium ions, so that the equilibrium adsorption amount of the sodium alginate-polyamidoxime composite hydrogel sphere uranium adsorption material obtained by the present invention is greater than that of the microporous polymer synthesized with sodium alginate and polyamidoxime as raw materials.

[0024] 3. The present invention uses sodium alginate, polyamidoximate and hyperbranched polyamide as raw materials, and Ca 2+ Cross-linking weaving, using glutaraldehyde for secondary cross-linking, and undergoing deep covalent cross-linking reaction, thereby producing a microporous spherical adsorption material with rich pores. The microporous adsorption material contains abundant amino and amidoxime functional groups, so that the amino-amidoxime bifunctional adsorption material obtained by the present invention exhibits excellent adsorption capacity for uranium, high adsorption rate and uranium ion selectivity; the adsorption material of the present invention has excellent adsorption capacity for uranium in K + , Na + ,Mg 2+ , Ca 2+ , Ba 2+ , Sr. 2+ ,Co 2+ , Cu 2+ It has a high selective adsorption capacity for uranium ions in aqueous solution with coexisting ions.

[0025] 4. In the present invention, a composite gel solution is first prepared using sodium alginate, polyamidoximes and hyperbranched polyamides as raw materials; the components of the gel solution contain a large number of amino and carboxyl groups, which provide a basis for the subsequent cross-linking reaction. In addition, the three polymer components in the gel solution contain a large number of amino and carboxyl groups, which make the material have good hydrophilicity and are easy to participate in the reaction for cross-linking, thereby improving the mechanical properties of the material; the gel solution obtained by the present invention is cross-linked twice; cross-linking is selected twice, and the first cross-linking is based on sodium alginate in the gel solution, and gel balls are formed by calcium ion cross-linking, so that the material has a stable three-dimensional porous structure, and the second cross-linking is cross-linked by glutaraldehyde to further enhance the stability of the material.

[0026] 5. In the present invention, after HA is added, the SA-PAO / HA gel sphere as a whole is obviously porous and has more abundant pores under the microscopic view. This is because the multi-branched structure in the hyperbranched polyamide molecule is connected to sodium alginate and polyamidoximine through the multi-branched structure during covalent cross-linking, so that the material forms disordered multi-branched long chains in three-dimensional space, thereby forming a three-dimensional network-supported gel system, so that the material realizes a porous structure during the secondary cross-linking molding process. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The infrared spectra of SA-PAO / HA, raw materials and SA-PAO prepared in Example 1 are shown in FIG.

[0028] Figure 2 This is a scanning electron micrograph of the SA-PAO / HA prepared in Example 1;

[0029] Figure 3 The relationship diagram between the uranium adsorption rate of SA-PAO / HA prepared in Example 1 and the solid-liquid ratio (the mass ratio of the adsorbent to the volume ratio of the adsorption solution);

[0030] Figure 4 Graph showing the removal rate of different cations by the adsorbent material; in the graph, SA-PAO / HA is the adsorbent material prepared in Example 1, and SA-PAO is the adsorbent material prepared in Example 2;

[0031] Figure 5 This is the relationship between the adsorption amount of U(VI) by SA-PAO / HA and the HA content. DETAILED DESCRIPTION

[0032] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any reasonable combination of the specific implementation modes.

[0033] Specific implementation method 1: The structural formula of the sodium alginate-polyamidoxime composite hydrogel spherical uranium adsorption material in this implementation method is:

[0034]

[0035] This implementation has the following beneficial effects:

[0036] 1. The sodium alginate-polyamidoxime composite hydrogel sphere uranium adsorption material of this embodiment contains abundant amino and amidoxime functional groups, exhibits excellent adsorption capacity for uranium, has high adsorption rate and uranium ion selectivity; has the highest adsorption capacity at pH 6, and has a high adsorption rate at concentration C 0 =100ppm, pH=6 uranium solution, the removal rate of uranium ions can reach more than 95% (the adsorption amount can reach more than 475mg / g).

[0037] 2. Due to the synergistic adsorption effect of amino and amidoxime groups, additional binding sites are provided and affinity is enhanced during the coordination process with uranium ions, thereby improving the adsorption efficiency and capacity of uranium ions, so that the equilibrium adsorption amount of the sodium alginate-polyamidoxime composite hydrogel sphere uranium adsorption material obtained in this embodiment is greater than that of the microporous polymer synthesized with sodium alginate and polyamidoxime as raw materials.

[0038] 3. This embodiment uses sodium alginate, polyamidoximate and hyperbranched polyamide as raw materials, and Ca 2+ Cross-linking weaving, using glutaraldehyde for secondary cross-linking, after deep covalent cross-linking reaction, a microporous spherical adsorption material with rich pores is produced. The microporous adsorption material contains rich amino and amidoxime functional groups, so that the amino-amidoxime bifunctional adsorption material obtained in this embodiment has excellent adsorption capacity for uranium, high adsorption rate and uranium ion selectivity; the adsorption material in this embodiment has excellent adsorption capacity for uranium in K + , Na + ,Mg 2+ , Ca 2+ , Ba 2+ , Sr. 2+ ,Co 2+ , Cu 2+ It has a high selective adsorption capacity for uranium ions in aqueous solution with coexisting ions.

[0039] 4. In this embodiment, a composite gel solution is first prepared using sodium alginate, polyamidoximes and hyperbranched polyamides as raw materials; the components of the gel solution contain a large number of amino and carboxyl groups, which provide a basis for the subsequent cross-linking reaction. In addition, the three polymer components in the gel solution contain a large number of amino and carboxyl groups, which make the material have good hydrophilicity and are easy to participate in the reaction for cross-linking, thereby improving the mechanical properties of the material; the gel solution obtained in this embodiment is cross-linked twice; cross-linking is selected twice, and the first cross-linking is based on sodium alginate in the gel solution, and gel balls are formed by calcium ion cross-linking, so that the material has a stable three-dimensional porous structure, and the second cross-linking further enhances the stability of the material through cross-linking with glutaraldehyde.

[0040] Specific implementation method 2: The preparation method of sodium alginate-polyamidoxime composite hydrogel spherical uranium adsorption material in this implementation method is carried out according to the following steps:

[0041] 1. Preparation of composite gel solution using polyamidoxime, sodium alginate and hyperbranched polyamide as raw materials:

[0042] Weighing sodium alginate powder and dissolving it in deionized water to obtain a sodium alginate solution; weighing polyamidoxime powder and dissolving it in a sodium hydroxide solution to obtain an alkaline polyamidoxime solution; weighing hyperbranched polyamide powder and dissolving it in deionized water to obtain a polyamide solution; adding the polyamidoxime solution and the polyamide solution to the sodium alginate solution and mechanically stirring them at room temperature, and then standing to obtain a composite gel solution;

[0043] The ratio of the mass of the sodium alginate powder to the volume of deionized water is (400-700) mg: (8-20) mL;

[0044] The ratio of the mass of the polyamidoxime powder to the volume of the sodium hydroxide solution is (0.15-1) g: (8-20) mL;

[0045] The concentration of the sodium hydroxide solution is 0.4-0.7 mol / L; the sodium hydroxide solution has a strong alkalinity, which is conducive to the dissolution of the polyamidoxime powder;

[0046] The ratio of the mass of the hyperbranched polyamide powder to the volume of deionized water is (0.25-2) g: (4.5-8) mL;

[0047] The mass ratio of sodium alginate to polyamidoxime is 1:(0.5-1.5); the mass ratio of polyamidoxime to hyperbranched polyamide is 1:(1.2-2.5); after using more hyperbranched polyamide, the rich negatively charged functional groups of the hyperbranched polyamide, such as amino, imino, acyloxy, etc., can improve the adsorption efficiency and capacity of uranium ions by providing additional binding sites and enhancing affinity, coordinately enhance the complexation of uranium ions by amidoxime groups, and then promote the improvement of the overall uranium adsorption amount. At the same time, more branched structures are the key to the formation of the porous structure of the gel ball.

[0048] The mechanical stirring time is 10-40 minutes, and the standing time is 15-40 minutes; standing after the stirring can eliminate bubbles and ensure that the gel balls formed during cross-linking are uniform.

[0049] 2. Cross-linking the composite gel solution obtained in step 1 twice to obtain sodium alginate-polyamidoximine composite hydrogel spheres;

[0050] The process of the double cross-linking is as follows: dropping the composite gel solution obtained in step 1 into a calcium ion solution for primary cross-linking molding, then filtering and washing with deionized water for several times to obtain gel balls; then placing the gel balls in a glutaraldehyde solution for secondary cross-linking molding, shaking during the secondary cross-linking molding process, then washing the gel balls with deionized water for several times, and finally freeze-drying to obtain a sodium alginate-polyamidooxime composite hydrogel ball uranium adsorption material;

[0051] The time of the primary cross-linking molding is 1-5 hours, and the calcium ion solution is a calcium chloride solution with a concentration of 2-4wt.%;

[0052] The secondary cross-linking molding time is 7-12 hours, and the mass fraction of the glutaraldehyde solution is 1.5-4%.

[0053] This embodiment has the following beneficial effects:

[0054] 1. The sodium alginate-polyamidoxime composite hydrogel sphere uranium adsorption material of this embodiment contains abundant amino and amidoxime functional groups, exhibits excellent adsorption capacity for uranium, has high adsorption rate and uranium ion selectivity; has the highest adsorption capacity at pH 6, and has a high adsorption rate at concentration C 0 =100ppm, pH=6 uranium solution, the removal rate of uranium ions can reach more than 95% (the adsorption amount can reach more than 475mg / g).

[0055] 2. Due to the synergistic adsorption effect of amino and amidoxime groups, additional binding sites are provided and affinity is enhanced during the coordination process with uranium ions, thereby improving the adsorption efficiency and capacity of uranium ions, so that the equilibrium adsorption amount of the sodium alginate-polyamidoxime composite hydrogel sphere uranium adsorption material obtained in this embodiment is greater than that of the microporous polymer synthesized with sodium alginate and polyamidoxime as raw materials.

[0056] 3. This embodiment uses sodium alginate, polyamidoximate and hyperbranched polyamide as raw materials, and Ca 2+ Cross-linking weaving, using glutaraldehyde for secondary cross-linking, after deep covalent cross-linking reaction, a microporous spherical adsorption material with rich pores is produced. The microporous adsorption material contains rich amino and amidoxime functional groups, so that the amino-amidoxime bifunctional adsorption material obtained in this embodiment has excellent adsorption capacity for uranium, high adsorption rate and uranium ion selectivity; the adsorption material in this embodiment has excellent adsorption capacity for uranium in K + , Na + ,Mg 2+ , Ca 2+ , Ba 2+ , Sr. 2+ ,Co 2+ , Cu 2+ It has a high selective adsorption capacity for uranium ions in aqueous solution with coexisting ions.

[0057] 4. In this embodiment, a composite gel solution is first prepared using sodium alginate, polyamidoximes and hyperbranched polyamides as raw materials; the components of the gel solution contain a large number of amino and carboxyl groups, which provide a basis for the subsequent cross-linking reaction. In addition, the three polymer components in the gel solution contain a large number of amino and carboxyl groups, which make the material have good hydrophilicity and are easy to participate in the reaction for cross-linking, thereby improving the mechanical properties of the material; the gel solution obtained in this embodiment is cross-linked twice; cross-linking is selected twice, and the first cross-linking is based on sodium alginate in the gel solution, and gel balls are formed by calcium ion cross-linking, so that the material has a stable three-dimensional porous structure, and the second cross-linking further enhances the stability of the material through cross-linking with glutaraldehyde.

[0058] Specific implementation method three: This implementation method is different from specific implementation method two in that: in step one, the ratio of the mass of the sodium alginate powder to the volume of deionized water is 500 mg:10 mL.

[0059] Specific embodiment 4: This embodiment differs from specific embodiment 2 in that: in step 1, the ratio of the mass of the polyamidooxime powder to the volume of the sodium hydroxide solution is 0.5 g:10 mL.

[0060] Specific implementation mode 5: This implementation mode is different from specific implementation mode 2 in that: the concentration of the sodium hydroxide solution in step 1 is 0.5 mol / L.

[0061] Specific implementation method 6: This implementation method is different from specific implementation method 2 in that: in step 1, the ratio of the mass of the hyperbranched polyamide powder to the volume of deionized water is 1 g:5 mL.

[0062] Specific embodiment seven: This embodiment differs from specific embodiment two in that: in step one, the mass ratio of sodium alginate to polyamidoxime is 1:1; the mass ratio of polyamidoxime to hyperbranched polyamide is 1:2.

[0063] Specific embodiment eight: This embodiment differs from specific embodiment two in that: the time for the one-time cross-linking molding in step two is 2 hours, and the calcium ion solution is a calcium chloride solution with a concentration of 2.5wt.%.

[0064] Specific implementation method 9: This implementation method is different from specific implementation method 2 in that: the time for the secondary cross-linking molding in step 2 is 9 hours, and the mass fraction of the glutaraldehyde solution is 2%.

[0065] Specific implementation method ten: This implementation method is different from specific implementation method two in that: the number of deionized water washing times in step two is 3-5 times.

[0066] Embodiment 1:

[0067] The preparation method of the sodium alginate-polyamidoxime composite hydrogel spherical uranium adsorbent of this embodiment is carried out according to the following steps:

[0068] 1. Preparation of composite gel solution using polyamidoxime, sodium alginate and hyperbranched polyamide as raw materials:

[0069] 500 mg of sodium alginate (SA) powder was weighed and dissolved in 10 mL of deionized water to obtain a sodium alginate solution; 500 mg of polyamidooxime (PAO) powder was weighed and dissolved in 10 mL of 0.5 mol / L sodium hydroxide solution to obtain an alkaline polyamidooxime solution; 1000 mg of hyperbranched polyamide (HA) powder was weighed and dissolved in 5 mL of deionized water to obtain a polyamide solution; the polyamidooxime solution and the alkaline polyamide solution were added to the sodium alginate solution and heated at room temperature at 500 r·min -1 The mixture was mechanically stirred at a speed of 25 min and allowed to stand for 40 min to obtain a composite gel solution;

[0070] 2. Cross-linking the composite gel solution obtained in step 1 twice to obtain sodium alginate-polyamidoximine composite hydrogel spheres;

[0071] The process of the double cross-linking is as follows: the composite gel liquid obtained in step 1 is dripped into a calcium chloride solution with a concentration of 2.5wt.% for primary cross-linking molding for 2 hours, and then filtered and washed with deionized water for 3 times to obtain gel balls; the gel balls are then placed in a glutaraldehyde solution with a mass fraction of 2% for secondary cross-linking molding for 9 hours, shaken during the secondary cross-linking molding process, and then washed with deionized water for 3 times, and finally freeze-dried to obtain a sodium alginate-polyamidooxime composite hydrogel ball uranium adsorption material (SA-PAO / HA).

[0072] The structural formula of the sodium alginate-polyamidoxime composite hydrogel spherical uranium adsorption material prepared in this embodiment is:

[0073]

[0074] In order to better understand the promoting effect of hyperbranched polyamide (HA) on amidoxime porous adsorbent and explore the role of the ratio of amino and amidoxime content and the microporous structure, an amidated porous polymer without HA (Example 2) and a SA-PAO / HA material prepared with 1000 mg HA (Example 1) were used as comparisons.

[0075] Embodiment 2:

[0076] 1. Preparation of composite gel solution using polyamidoxime, sodium alginate and hyperbranched polyamide as raw materials:

[0077] Weigh 500 mg of sodium alginate (SA) powder and dissolve it in 10 mL of deionized water to obtain a sodium alginate solution; weigh 500 mg of polyamidooxime (PAO) powder and dissolve it in 10 mL of 0.5 mol / L sodium hydroxide solution to obtain an alkaline polyamidooxime solution; add the alkaline polyamidooxime solution to the sodium alginate solution and heat it at room temperature at 500 r·min -1 The mixture was mechanically stirred at a speed of 25 min and allowed to stand for 40 min to obtain a composite gel solution;

[0078] 2. Cross-linking the composite gel solution obtained in step 1 twice to obtain sodium alginate-polyamidoximine composite hydrogel spheres;

[0079] The process of the double cross-linking is as follows: the composite gel liquid obtained in step 1 is dripped into a calcium chloride solution with a concentration of 2.5wt.% for primary cross-linking molding for 2 hours, then filtered and washed with deionized water for 3 times to obtain gel balls; then the gel balls are placed in a glutaraldehyde solution with a mass fraction of 2% for secondary cross-linking molding for 9 hours, shaken during the secondary cross-linking molding process, then washed with deionized water for 3 times, and finally freeze-dried to obtain gel balls (SA-PAO).

[0080] experiment:

[0081] ①. Conducting a laboratory uranium adsorption experiment: Weigh 0.01 g of SA-PAO / HA prepared in Example 1, place it in a 250 mL conical flask, and then add 50 mL of a uranium solution (uranyl nitrate solution, adsorption solution) with a pH of 6. After adsorption for a certain period of time at 25° C., separate the adsorbent SA-PAO / HA with a porous filter membrane to obtain an adsorbed uranium solution. Then, use inductively coupled plasma atomic emission spectroscopy (ICP-AES) to determine the concentration of U(VI) in the uranyl nitrate solution before and after adsorption, and calculate the adsorption amount of U(VI) by SA-PAO / HA according to formula (1): e ;

[0082]

[0083] In formula (1), C 0 is the concentration of uranium solution before adsorption (mg / L), C e is the concentration of uranium solution after adsorption equilibrium (mg / L), V is the volume of adsorption solution (L), and m is the mass of adsorbent (g);

[0084] ②. Coexisting ion competitive adsorption experiment: First, prepare the coexisting ion solution: weigh the nitrate of potassium ion, sodium ion, calcium ion, magnesium ion, copper ion, strontium ion, cobalt ion and barium ion in the same amount as uranyl ion on an electronic balance, place it in a 250mL beaker, add 100mL deionized water to dissolve, ultrasonicate for 15min until completely dissolved, then transfer to a 1000mL volumetric flask, set to volume for use. Then add it to a centrifuge tube, then add the adsorbent, stir at 25℃, and perform ICP-AES to determine the uranium concentration in the supernatant after adsorption by the adsorbent. Use formula (1) to calculate the removal rate of various ions by the adsorbent.

[0085] ③. Adsorption experiment of SA-PAO without adding HA: 10 mg of the gel ball (SA-PAO) prepared in Example 2 was weighed and placed in a 250 ml conical flask, and 10 ml of uranium solution (uranyl nitrate solution) with a pH of 6 was added. After adsorption for a specific time at 25° C., the adsorbent was separated by a porous filter membrane to obtain the adsorbed uranium solution. The concentration of U(VI) in the uranium solution before and after adsorption was then determined by ICP-AES, and the adsorption amount of U(VI) by the adsorbent was calculated according to formula (1): e The concentration of U(VI) in the uranyl nitrate solution before and after adsorption was measured, and the adsorption amount of U(VI) was calculated according to formula (1). The adsorption amount of Example 1 was 475.35 mg / g, and the adsorption amount of Example 2 was 374.41 mg / g. Compared with Example 1, Example 2 had a lower adsorption amount, which fully demonstrated that the porous structure exhibited by the introduction of polyamide in Example 1 and the synergistic effect of amino and amidoxime groups were conducive to the improvement of the adsorption amount.

[0086] Figure 1 IR spectra of SA-PAO / HA, raw materials and SA-PAO prepared in Example 1; Figure 1 It is known that 938cm -1 The characteristic peak at 1658 cm-1 can be attributed to the stretching vibration peak of NO in the amidoxime group. -1 and 1388cm -1 The characteristic peaks at 1030cm -1 The stretching vibration peak of COC at 1104 cm -1 The CN absorption peak of tertiary amine appears at , proving the introduction of HA. This shows that Example 1 successfully prepared the uranium adsorption material with amino-amidoxime bifunctional groups.

[0087] Figure 2 is a scanning electron micrograph of SA-PAO / HA prepared in Example 1; Figure 2As shown, the gel sphere appears to be an obvious porous sphere as a whole and has more abundant pores under the microscopic view.

[0088] Figure 3 The relationship between the uranium adsorption rate and the solid-liquid ratio (the mass ratio of the adsorbent to the volume ratio of the adsorption solution) of the SA-PAO / HA prepared in Example 1 is shown in FIG. Figure 3 It can be seen that with the increase of solid-liquid ratio, the removal rate of uranyl ions gradually increases. When the solid-liquid ratio increases to 0.8g / L, the removal rate curve almost tends to equilibrium.

[0089] Figure 4 Removal rate of adsorbent materials for different cations; competitive adsorption with common cations in seawater shows that the adsorbent still maintains excellent uranium selectivity (removal rate exceeds 80%) in the presence of multiple interfering ions.

[0090] Embodiment 3:

[0091] The preparation method of the sodium alginate-polyamidoxime composite hydrogel spherical uranium adsorbent of this embodiment is carried out according to the following steps:

[0092] 1. Preparation of composite gel solution using polyamidoxime, sodium alginate and hyperbranched polyamide as raw materials:

[0093] 500 mg of sodium alginate (SA) powder was weighed and dissolved in 10 mL of deionized water to obtain a sodium alginate solution; 500 mg of polyamidooxime (PAO) powder was weighed and dissolved in 10 mL of 0.5 mol / L sodium hydroxide solution to obtain an alkaline polyamidooxime solution; 500 mg of hyperbranched polyamide (HA) powder was weighed and dissolved in 5 mL of deionized water to obtain a polyamide solution; the polyamidooxime solution and the alkaline polyamide solution were added to the sodium alginate solution and heated at room temperature at 500 r·min -1 The mixture was mechanically stirred at a speed of 25 min and allowed to stand for 40 min to obtain a composite gel solution;

[0094] 2. Cross-linking the composite gel solution obtained in step 1 twice to obtain sodium alginate-polyamidoximine composite hydrogel spheres;

[0095] The process of the double cross-linking is as follows: the composite gel liquid obtained in step 1 is dripped into a calcium chloride solution with a concentration of 2.5wt.% for primary cross-linking molding for 2 hours, and then filtered and washed with deionized water for 3 times to obtain gel balls; the gel balls are then placed in a glutaraldehyde solution with a mass fraction of 2% for secondary cross-linking molding for 9 hours, shaken during the secondary cross-linking molding process, and then washed with deionized water for 3 times, and finally freeze-dried to obtain a sodium alginate-polyamidooxime composite hydrogel ball uranium adsorption material (SA-PAO / HA).

[0096] 0, 250, 750, 1250 and 1500 mg of hyperbranched polyamide (HA) powder were weighed respectively and dissolved in 5 mL of deionized water to obtain 5 polyamide solutions. The other processes and parameters were the same as those in Example 3, and uranium adsorption materials with different hyperbranched polyamide (HA) contents were prepared according to the process of Example 3.

[0097] The molecular weight of the polyamidoximes used in Examples 1 and 3 is 100,000 to 200,000;

[0098] Figure 5 This is the relationship between the adsorption amount of U(VI) by SA-PAO / HA and the HA content. As the HA content gradually increases, the increment of the unit uranium adsorption of SA-PAO / HA shows a trend of first increasing and then decreasing, but the adsorption amount increases overall and reaches the maximum at 750 mg. This is because the rich negatively charged functional groups in HA, such as amino, imino, and acyloxy groups, can coordinate the complexation of uranium ions with amidoxime groups, thereby promoting the increase in the overall uranium adsorption amount. At the same time, excessive addition of HA causes the amidoxime groups to be excessively diluted, resulting in a decrease in the adsorption effect.

Claims

1. A sodium alginate-polyamidoxime composite hydrogel spherical uranium adsorption material, characterized in that: The structural formula of sodium alginate-polyamidoximine composite hydrogel sphere uranium adsorption material is:

2. The method for preparing the sodium alginate-polyamidoxime composite hydrogel spherical uranium adsorption material according to claim 1, characterized in that: The preparation method is carried out according to the following steps:

1. Preparation of composite gel solution using polyamidoxime, sodium alginate and hyperbranched polyamide as raw materials: Weighing sodium alginate powder and dissolving it in deionized water to obtain a sodium alginate solution; weighing polyamidoxime powder and dissolving it in a sodium hydroxide solution to obtain an alkaline polyamidoxime solution; weighing hyperbranched polyamide powder and dissolving it in deionized water to obtain a polyamide solution; adding the polyamidoxime solution and the polyamide solution to the sodium alginate solution and mechanically stirring them at room temperature, and then standing to obtain a composite gel solution; The ratio of the mass of the sodium alginate powder to the volume of deionized water is (400-700) mg: (8-20) mL; The ratio of the mass of the polyamidoxime powder to the volume of the sodium hydroxide solution is (0.15-1) g: (8-20) mL; The concentration of the sodium hydroxide solution is 0.4-0.7 mol / L; The ratio of the mass of the hyperbranched polyamide powder to the volume of deionized water is (0.25-2) g: (4.5-8) mL; The mass ratio of sodium alginate to polyamidoxime is 1:(0.5-1.5); the mass ratio of polyamidoxime to hyperbranched polyamide is 1:(1.2-2.5); The mechanical stirring time is 10-40 minutes, and the standing time is 15-40 minutes; 2. Cross-linking the composite gel solution obtained in step 1 twice to obtain sodium alginate-polyamidoximine composite hydrogel spheres; The process of the double cross-linking is as follows: dropping the composite gel solution obtained in step 1 into a calcium ion solution for primary cross-linking, then filtering and washing with deionized water for several times to obtain gel balls; then placing the gel balls in a glutaraldehyde solution for secondary cross-linking, shaking during the secondary cross-linking, then washing the gel balls with deionized water for several times, and finally freeze-drying to obtain a sodium alginate-polyamidooxime composite hydrogel ball uranium adsorption material; The time of the primary cross-linking molding is 1-5 hours, and the calcium ion solution is a calcium chloride solution with a concentration of 2-4wt.%; The secondary cross-linking molding time is 7-12 hours, and the mass fraction of the glutaraldehyde solution is 1.5-4%.

3. The method for preparing the sodium alginate-polyamidoxime composite hydrogel spherical uranium adsorption material according to claim 1, characterized in that: In step 1, the ratio of the mass of the sodium alginate powder to the volume of deionized water is 500 mg:10 mL.

4. The method for preparing the sodium alginate-polyamidoxime composite hydrogel spherical uranium adsorption material according to claim 1, characterized in that: The ratio of the mass of the polyamidooxime powder in step 1 to the volume of the sodium hydroxide solution is 0.5 g:10 mL.

5. The method for preparing the sodium alginate-polyamidoxime composite hydrogel spherical uranium adsorption material according to claim 1, characterized in that: The concentration of the sodium hydroxide solution in step 1 is 0.5 mol / L.

6. The method for preparing the sodium alginate-polyamidoxime composite hydrogel spherical uranium adsorption material according to claim 1, characterized in that: In step 1, the ratio of the mass of the hyperbranched polyamide powder to the volume of deionized water is 1 g:5 mL.

7. The method for preparing the sodium alginate-polyamidoxime composite hydrogel spherical uranium adsorption material according to claim 1, characterized in that: In step 1, the mass ratio of sodium alginate to polyamidoximine is 1:1; the mass ratio of polyamidoximine to hyperbranched polyamide is 1:

2.

8. The method for preparing the sodium alginate-polyamidoxime composite hydrogel spherical uranium adsorption material according to claim 1, characterized in that: The time for the primary cross-linking molding in step 2 is 2 hours, and the calcium ion solution is a calcium chloride solution with a concentration of 2.5 wt.%.

9. The method for preparing the sodium alginate-polyamidoxime composite hydrogel spherical uranium adsorption material according to claim 1, characterized in that: The time for the secondary cross-linking molding in step 2 is 9 hours, and the mass fraction of the glutaraldehyde solution is 2%.

10. The method for preparing the sodium alginate-polyamidoxime composite hydrogel spherical uranium adsorption material according to claim 1, characterized in that: The deionized water washing times in step 2 are 3-5 times.