Hydrotalcite-derived methane cracking catalyst as well as preparation method and application thereof
Through the preparation of hydrotalcite-derived catalysts, the use of NiCr alloy to reduce metal sintering is solved, and the problem of poor stability of methane cracking catalysts at high temperatures is optimized. By optimizing the electromagnetic wave absorption performance of the waste catalyst, the efficient application of catalysts and the effectiveness of carbon nanotubes are achieved. use.
Patent Information
- Application Number
- CN202410933309.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-05
AI Technical Summary
Existing methane cracking catalysts are prone to carbon decompression at high temperatures, and particle sintering leads to poor catalytic stability, and metal contamination of carbon nanomaterials in the spent catalysts is difficult to remove, limiting its application range.
Using hydrotalcite-derived catalyst, precipitation reaction is carried out through aluminum precursor, nickel precursor and chromium precursor, urea is added as a reducing agent to form a NiCr alloy, reduce the degree of metal sintering, and reduce it through a mixed gas of hydrogen and argon to prepare A catalyst with good sintering resistance is produced.
The uniform dispersion of Ni and Cr elements in the catalyst is achieved, the anti-sintering performance of the catalyst is improved, multi-walled carbon nanotubes with smaller diameters are generated, and the electromagnetic wave absorption performance of the waste catalyst is optimized, suitable for methane cracking and electromagnetic wave absorption applications.
Smart Images

Figure CN118892841A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of catalyst synthesis, and relates to a methane cracking catalyst and a preparation method and application thereof, and in particular to a hydrotalcite-derived methane cracking catalyst and a preparation method and application thereof. Background Art
[0002] Methane cracking to produce hydrogen can simultaneously produce hydrogen and high-value-added carbon nanomaterials without the production of carbon oxides. It has become an attractive alternative way to obtain high-purity hydrogen and has broad application prospects. In the process of industrialization, the selection of suitable catalysts is crucial to improving the efficiency of methane cracking to produce hydrogen. Transition metals Ni, Co and Fe have been widely used in the study of methane cracking due to their high activity and low cost. Among them, Ni has attracted the most attention due to its higher activity at low temperatures. However, Ni catalysts still have the challenges of rapid carbon deposition and deactivation at high temperatures and particle sintering, resulting in poor catalytic stability.
[0003] Layered double hydroxides (LDHs) are widely used as heterogeneous catalysts due to their diverse chemical composition, controllable structure and good stability. LDHs are an ionic layered compound composed of divalent and trivalent metal cations within the layer and interlayer anions. Through calcination and reduction treatment, the inherent topological directional phase transition from the LDHs matrix to the supported metal nanoparticles ensures a strong anchoring effect, and a stable catalyst with uniform and well-dispersed particles can be obtained. [Cíntia Quissini Salib, Oscar W. Perez-Lopez. Fuel 364 (2024) 131120.] NiAl hydrotalcite was used as a precursor to prepare Ni / Al2O3 catalyst for methane cracking. Sintering occurred in the reaction, causing particle agglomeration and deactivation, resulting in low catalytic stability. CN112705208 A discloses a hydrotalcite-derived NiGaAl catalyst for methane cracking and hydrogen production, but its hydrogen yield is less than 55%.
[0004] Carbon nanotubes are another product of the methane cracking hydrogen production reaction with unique chemical, mechanical and electronic properties. If these carbon nanomaterials are commercially applied, it will greatly improve the market competitiveness of the methane cracking process. However, the carbon nanomaterials produced by methane cracking are inevitably contaminated by the metals wrapped therein. In many applications, such as carbon electrodes, the metal content in the carbon needs to be reduced to the ppm level, but it is extremely challenging to purify carbon nanomaterials from methane cracking waste catalysts. Therefore, the application areas of these carbon nanomaterials have to be reconsidered.
[0005] Therefore, it is necessary to develop a sintering-resistant methane cracking catalyst and find ideas for the direct application of spent catalysts. Summary of the invention
[0006] In order to solve the technical problems existing in the prior art, the present invention provides a hydrotalcite-derived methane cracking catalyst and a preparation method and application thereof. The active components and additives in the catalyst are evenly dispersed, and the catalyst has good anti-sintering performance, and the used waste catalyst has excellent electromagnetic wave absorption performance.
[0007] In order to achieve the above technical effects, the present invention adopts the following technical solutions:
[0008] One of the purposes of the present invention is to provide a hydrotalcite-derived methane cracking catalyst, which comprises an Al2O3 carrier, and an active component and an auxiliary agent supported on the Al2O3 carrier, wherein the active component is Ni and the auxiliary agent is Cr.
[0009] As a preferred technical solution of the present invention, the molar ratio of the total molar number of active components and auxiliary agents to the aluminum element in the Al2O3 carrier is 2.5 to 3.5, such as 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4 or 3.5, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0010] As a preferred technical solution of the present invention, the molar ratio of the active component to the auxiliary agent is 1:19 to 2:3, such as 1:19, 1:18, 1:15, 1:12, 1:10, 1:8, 1:5, 1:3, 2:5, 2:4 or 2:3, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0011] The second object of the present invention is to provide a method for preparing hydrotalcite-derived methane by cracking provided in the first object of the present invention, the preparation method comprising:
[0012] A hydrotalcite precursor is prepared by carrying out precipitation reaction with an aluminum precursor, a nickel precursor and a chromium precursor;
[0013] The hydrotalcite precursor is subjected to a reduction reaction to obtain the catalyst.
[0014] As a preferred technical solution of the present invention, urea is used as a reducing agent in the precipitation reaction.
[0015] Preferably, the precipitation reaction temperature is 100-150°C, and the time is 20-30h. The temperature may be 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C or 150°C, and the time may be 20h, 21h, 22h, 23h, 24h, 25h, 26h, 27h, 28h, 29h or 30h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0016] As a preferred technical solution of the present invention, the precipitation reaction is a hydrothermal reaction.
[0017] As a preferred technical solution of the present invention, the reduction reaction uses a mixed gas of hydrogen and argon as a reducing agent.
[0018] As a preferred technical solution of the present invention, the volume content of hydrogen in the mixed gas of hydrogen and argon is 5-20%, such as 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0019] As a preferred technical solution of the present invention, the temperature of the reduction reaction is 700-1000°C and the time is 2-6 hours. The temperature can be 700°C, 750°C, 800°C, 850°C, 900°C, 950°C or 1000°C, etc., but is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0020] The third object of the present invention is to provide an application of the hydrotalcite-derived methane cracking catalyst provided in the first object of the present invention, wherein the catalyst is used for methane cracking to prepare hydrogen and carbon nanomaterials.
[0021] Compared with the prior art, the present invention has at least the following beneficial effects:
[0022] (1) The present invention provides a hydrotalcite-derived methane cracking catalyst and a preparation method and application thereof, wherein the Ni and Cr elements in the catalyst are uniformly dispersed during the preparation process, the average grain size of the NiCr alloy is 7 to 10 nm, and the catalyst has the characteristics of uniform composition and adjustable structure;
[0023] (2) The present invention provides a hydrotalcite-derived methane cracking catalyst and its preparation method and application. The catalyst exhibits good anti-sintering performance during the methane cracking reaction. Compared with the NiAl catalyst, the addition of Cr greatly reduces the degree of metal sintering, and multi-walled carbon nanotubes with smaller diameters can be obtained by reaction.
[0024] (3) The present invention provides a hydrotalcite-derived methane cracking catalyst and a preparation method and application thereof. The waste catalyst obtained after use has excellent electromagnetic wave absorption performance due to the presence of more defects and the synergistic effect of carbon nanotubes and metal particles. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The XRD diagrams of the hydrotalcite-derived methane cracking catalysts prepared in the examples and comparative examples of the present invention;
[0026] Figure 2A graph showing the hydrogen yield over time when the catalysts prepared in the examples and comparative examples of the present invention are applied to hydrogen production by cracking methane;
[0027] Figure 3 This is a TEM image of the hydrotalcite-derived methane cracking catalyst prepared in Example 1 of the present invention;
[0028] Figure 4 This is a graph showing the electromagnetic wave absorption performance of the spent catalyst after methane cracking reaction of the catalyst prepared in Invention Example 1.
[0029] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims. DETAILED DESCRIPTION
[0030] The technical solution of the present invention is further described below through specific implementation methods.
[0031] A specific embodiment of the present invention provides a hydrotalcite-derived methane cracking catalyst, which includes an Al2O3 carrier, and an active component and an auxiliary agent supported on the Al2O3 carrier, wherein the active component is Ni and the auxiliary agent is Cr.
[0032] In the present invention, the catalyst uses Al2O3 as a carrier and Ni as an active component. By adding Cr as an additive, the degree of metal sintering is greatly reduced, and methane cracking reaction is catalyzed to obtain multi-walled carbon nanotubes with smaller diameters.
[0033] In a specific embodiment of the present invention, the hydrotalcite-derived methane cracking catalyst uses NiCr alloy as the active phase.
[0034] A specific embodiment of the present invention provides a method for preparing a hydrotalcite-derived methane cracking catalyst, the preparation method comprising:
[0035] A hydrotalcite precursor is prepared by carrying out precipitation reaction with an aluminum precursor, a nickel precursor and a chromium precursor;
[0036] The hydrotalcite precursor is subjected to a reduction reaction to obtain the catalyst.
[0037] In a specific embodiment of the present invention, the aluminum precursor is preferably Al(NO3)3·9H2O, the nickel precursor is preferably Ni(NO3)2·6H2O, and the chromium precursor is preferably Cr(NO3)3·9H2O. The above precursors are only simple examples, and other suitable aluminum precursors, nickel precursors and chromium precursors can also be applied to this application.
[0038] In one specific embodiment of the present invention, after the aluminum precursor, the nickel precursor and the chromium precursor are dissolved in deionized water, a precipitant (urea) is added to the precursor solution for further mixing.
[0039] In a specific embodiment of the present invention, the ratio of the aluminum precursor, the nickel precursor and the chromium precursor is adjusted according to the total molar ratio of the active components and the auxiliary agents in the catalyst and the molar ratio of the aluminum element in the Al2O3 carrier, and the molar ratio of the active components to the auxiliary agents, and is not specifically limited here.
[0040] In a specific embodiment of the present invention, the precipitant (urea) should be added in excess, specifically 3 to 10 times, preferably 5 times, the total molar amount of metal ions in the aluminum precursor, the nickel precursor and the chromium precursor.
[0041] In one specific embodiment of the present invention, the precipitation reaction is carried out in a hydrothermal reactor.
[0042] In one embodiment of the present invention, the hydrotalcite precursor is Ni 3-x Cr x Al-based hydrotalcite, wherein x ranges from 0 to 1.2, excluding 0.
[0043] In one specific embodiment of the present invention, the obtained hydrotalcite precursor is washed and dried before the reduction reaction. The washing method may be washing with deionized water and anhydrous ethanol alternately, and the drying condition may be drying at 80° C. for 12 hours. The above washing method and drying conditions are only examples, which can be selected according to the conditions of the prepared hydrotalcite precursor and are not further limited here.
[0044] In one embodiment of the present invention, the introduction rate of hydrogen and argon in the reduction reaction can be specifically adjusted according to the reaction conditions, and is not specifically limited here. For example, the introduction rate of hydrogen and argon can be 100 mL / min.
[0045] In a specific embodiment of the present invention, the heating rate of the reduction reaction can be specifically adjusted according to the reaction conditions, and is not specifically limited here. For example, the heating rate of the reduction reaction can be 5°C / min.
[0046] In a specific embodiment of the present invention, the waste catalyst generated after the hydrotalcite-derived methane cracking catalyst provided by the present invention is subjected to a methane cracking reaction can be used for electromagnetic wave absorption.
[0047] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:
[0048] Example 1
[0049] This embodiment provides a method for preparing a hydrotalcite-derived methane cracking catalyst, the preparation method comprising:
[0050] 8.1mmol(NO3)2·6H2O, 0.9mmolCr(NO3)3·9H2O and 3mmolAl(NO3)3·9H2O were added to 70ml of deionized water, and then 60mmol of urea was added to the above solution. After vigorous stirring for 1h, the mixed solution was transferred to a 100ml polytetrafluoroethylene-lined stainless steel hydrothermal autoclave and reacted at 110℃ for 24h. The solid product was obtained by centrifugation, washed several times with deionized water and anhydrous ethanol, and dried at 80℃ for 12h to obtain Ni 2.7 Cr 0.3 Al LDHs;
[0051] 400 mg of Ni was heated at a rate of 5 °C / min in a continuous 10% H2 / Ar atmosphere. 2.7 Cr 0.3 Al LDHs were heated to 800 °C and maintained for 4 h. The obtained catalysts were labeled as Ni 2.7 Cr 0.3 Al.
[0052] Example 2
[0053] This embodiment provides a method for preparing a hydrotalcite-derived methane cracking catalyst, the preparation method comprising:
[0054] 8.55mmol(NO3)2·6H2O, 0.45mmolCr(NO3)3·9H2O and 3mmolAl(NO3)3·9H2O were added to 70ml of deionized water, and then 60mmol of urea was added to the above solution. After vigorous stirring for 1h, the mixed solution was transferred to a 100ml polytetrafluoroethylene-lined stainless steel hydrothermal autoclave and reacted at 110℃ for 24h. The solid product was obtained by centrifugation, washed several times with deionized water and anhydrous ethanol, and dried at 80℃ for 12h to obtain Ni 2.85 Cr 0.15 Al LDHs;
[0055] 400 mg of Ni was heated at a rate of 5 °C / min in a continuous 10% H2 / Ar atmosphere. 2.85 Cr 0.15 Al LDHs were heated to 800 °C and maintained for 4 h. The obtained catalysts were labeled as Ni 2.85 Cr 0.15 Al.
[0056] Example 3
[0057] This embodiment provides a method for preparing a hydrotalcite-derived methane cracking catalyst, the preparation method comprising:
[0058] 7.2mmol(NO3)2·6H2O, 1.8mmolCr(NO3)3·9H2O and 3mmolAl(NO3)3·9H2O were added to 70ml of deionized water, and then 60mmol of urea was added to the above solution. After vigorous stirring for 1h, the mixed solution was transferred to a 100ml polytetrafluoroethylene-lined stainless steel hydrothermal autoclave and reacted at 110℃ for 24h. The solid product was obtained by centrifugation, washed several times with deionized water and anhydrous ethanol, and dried at 80℃ for 12h to obtain Ni 2.4 Cr 0.6 Al LDHs;
[0059] 400 mg of Ni was heated at a rate of 5 °C / min in a continuous 10% H2 / Ar atmosphere. 2.4 Cr 0.6 Al LDHs were heated to 800 °C and maintained for 4 h. The obtained catalysts were labeled as Ni 2.4 Cr 0.6 Al.
[0060] Example 4
[0061] This embodiment provides a method for preparing a hydrotalcite-derived methane cracking catalyst, the preparation method comprising:
[0062] 5.4mmol(NO3)2·6H2O, 3.6mmolCr(NO3)3·9H2O and 3mmolAl(NO3)3·9H2O were added to 70ml of deionized water, and then 60mmol of urea was added to the above solution. After vigorous stirring for 1h, the mixed solution was transferred to a 100ml polytetrafluoroethylene-lined stainless steel hydrothermal autoclave and reacted at 110℃ for 24h. The solid product was obtained by centrifugation, washed several times with deionized water and anhydrous ethanol, and dried at 80℃ for 12h to obtain Ni 1.8 Cr 1.2 Al LDHs;
[0063] 400 mg of Ni was heated at a rate of 5 °C / min in a continuous 10% H2 / Ar atmosphere. 1.8 Cr 1.2 Al LDHs were heated to 800 °C and maintained for 4 h. The obtained catalyst was labeled as Ni 1.8 Cr 1.2 Al.
[0064] Example 5
[0065] This embodiment provides a method for preparing a hydrotalcite-derived methane cracking catalyst, the preparation method comprising:
[0066] 8.1mmol(NO3)2·6H2O, 0.9mmolCr(NO3)3·9H2O and 3mmolAl(NO3)3·9H2O were added to 70ml of deionized water, and then 60mmol of urea was added to the above solution. After vigorous stirring for 1h, the mixed solution was transferred to a 100ml polytetrafluoroethylene-lined stainless steel hydrothermal autoclave and reacted at 100℃ for 30h. The solid product was obtained by centrifugation, washed several times with deionized water and anhydrous ethanol, and dried at 80℃ for 12h to obtain Ni 2.7 Cr 0.3 Al LDHs;
[0067] 400 mg of Ni was heated at a rate of 5 °C / min in a continuous 10% H2 / Ar atmosphere. 2.7 Cr 0.3 Al LDHs were heated to 700 °C and maintained for 6 h. The obtained catalysts were labeled as Ni 2.7 Cr 0.3 Al.
[0068] Example 6
[0069] This embodiment provides a method for preparing a hydrotalcite-derived methane cracking catalyst, the preparation method comprising:
[0070] 8.1mmol(NO3)2·6H2O, 0.9mmolCr(NO3)3·9H2O and 3mmolAl(NO3)3·9H2O were added to 70ml of deionized water, and then 60mmol of urea was added to the above solution. After vigorous stirring for 1h, the mixed solution was transferred to a 100ml polytetrafluoroethylene-lined stainless steel hydrothermal autoclave and reacted at 150℃ for 20h. The solid product was obtained by centrifugation, washed several times with deionized water and anhydrous ethanol, and dried at 80℃ for 12h to obtain Ni 2.7 Cr 0.3 Al LDHs;
[0071] 400 mg of Ni was heated at a rate of 5 °C / min in a continuous 10% H2 / Ar atmosphere. 2.7 Cr 0.3 Al LDHs were heated to 1000 °C and maintained for 2 h. The obtained catalysts were labeled as Ni 2.7 Cr 0.3 Al.
[0072] Comparative Example 1
[0073] This comparative example provides a method for preparing a methane cracking catalyst, the preparation method comprising:
[0074] 9mmol(NO3)2·6H2O and 3mmolAl(NO3)3·9H2O were added to 70ml of deionized water, and then 60mmol of urea was added to the above solution. After vigorous stirring for 1h, the mixed solution was transferred to a 100ml polytetrafluoroethylene-lined stainless steel hydrothermal autoclave and reacted at 110℃ for 24h. The solid product was obtained by centrifugation, washed several times with deionized water and anhydrous ethanol, and dried at 80℃ for 12h to obtain Ni3Al LDHs;
[0075] 400 mg of Ni3Al LDHs were heated to 800°C at a heating rate of 5°C / min under a continuous 10% H2 / Ar atmosphere and kept at that temperature for 4 h. The obtained catalyst was labeled as Ni3Al.
[0076] Comparative Example 2
[0077] In this comparative example, except that Cr(NO3)3·9H2O is replaced by Ga(NO3)3·9H2O of an equal amount, the other conditions are the same as those in Example 1.
[0078] The catalysts provided in Examples 1-6 and Comparative Examples 1 and 2 were evaluated for their methane cracking performance in a horizontally placed quartz tube reactor. First, 100 mg of the above catalysts with 40-60 mesh and 1 g of quartz sand were mixed evenly and placed in the middle of the reaction tube, and the catalysts were fixed with quartz wool. Before the test, the reactor was heated at 10 °C min in a 30 mL / min N2 gas flow. -1 The reactor was heated to 700°C at a heating rate of 1000 °C, and then the gas was replaced with 10% CH4 / Ar at 30 mL / min, and a methane cracking experiment was carried out for 360 minutes. After the reaction was completed, when the reactor was cooled to room temperature in the N2 flow, the spent catalyst in the quartz tube was collected. During the reaction, a 3400 gas chromatograph equipped with a TCD and FID detector was used to analyze the gas composition.
[0079] The waste catalysts of Comparative Example 1, Example 4 and Example 1 at different reaction temperatures were directly used for electromagnetic parameter testing, and the complex dielectric constant and magnetic permeability of the waste catalysts were tested in the frequency range of 2 to 18 GHz using a network analyzer (Agilent E5071C: 300 kHz to 20 GHz). Paraffin was used as a binder, and the mass fraction of the waste catalyst was 20 wt%.
[0080] The hydrogen yields of Examples 1-6 and Comparative Examples 1 and 2 after methane cracking reaction at 700° C. for 150 min are shown in Table 1.
[0081] Table 1
[0082] catalyst Hydrogen yield (%) Example 1 81.7 Example 2 68.6 Example 3 77.4 Example 4 69.8 Example 5 76.5 Example 6 78.8 Comparative Example 1 35.5 Comparative Example 2 65.2
[0083] In Examples 1-4, the alloy catalyst prepared in Comparative Example 1 after reduction of the NiCrAl hydrotalcite precursor was characterized by X-ray diffraction (XRD). The characterization results are as follows: Figure 1 All the reduced samples showed diffraction peaks belonging to the nickel crystal phase at 2θ=44.5°(111), 51.8°(200), and 76.3°(220) (JCPDS PDF#04-0850). Figure 2 For you 3- x Cr x The catalytic activity of Al catalyst for methane decomposition within 360 min reaction time. When the Cr content is 0.3, Ni 2.7 Cr 0.3 The Al catalyst was stable for 200 min with a hydrogen yield of not less than 80%, showing good catalytic stability. Figure 3 Ni after reaction 2.7 Cr 0.3 TEM image of Al spent catalyst, indicating that a large amount of carbon nanotubes were produced. Figure 4 Ni with different thicknesses after catalytic reaction in Example 1 2.7 Cr 0.3 The electromagnetic wave reflection loss value of Al waste catalyst. When the thickness is 1.6mm, the minimum reflection loss value at 15.3GHz is -44.5dB, and the effective absorption bandwidth reaches 4.7GHz (13.3-18Ghz). The results show that Ni at a reaction temperature of 620℃ 2.7 Cr 0.3 Al spent catalyst has good electromagnetic wave absorption performance.
[0084] Compared with Comparative Example 1, Examples 1-6 have relatively higher stability because the addition of Cr increases the specific surface area of the catalyst and promotes the reduction performance of metal Ni.
[0085] Compared with Comparative Example 2, Examples 1-6 have higher activities because the addition of Cr makes Ni have a suitable particle size and good metal dispersion compared with Ga, thus having optimal catalytic activity and stability.
[0086] The applicant declares that the present invention illustrates the detailed structural features of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed structural features, that is, it does not mean that the present invention must rely on the above-mentioned detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0087] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0088] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0089] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A hydrotalcite-derived methane cracking catalyst, characterized in that: The catalyst comprises an Al2O3 carrier, and an active component and an auxiliary agent supported on the Al2O3 carrier, wherein the active component is Ni and the auxiliary agent is Cr.
2. The catalyst according to claim 1, characterized in that The molar ratio of the total molar number of the active components and the auxiliary agent to the aluminum element in the Al2O3 carrier is 2.5 to 3.
5.
3. The water catalyst according to claim 1, characterized in that The molar ratio of the active component to the auxiliary agent is 1:19 to 2:
3.
4. A method for preparing a hydrotalcite-derived methane cracking catalyst according to any one of claims 1 to 3, characterized in that: The preparation method comprises: A hydrotalcite precursor is prepared by carrying out precipitation reaction with an aluminum precursor, a nickel precursor and a chromium precursor; The hydrotalcite precursor is subjected to a reduction reaction to obtain the catalyst.
5. The preparation method according to claim 4, characterized in that: The precipitation reaction uses urea as a precipitant; Preferably, the precipitation reaction is carried out at a temperature of 100 to 150° C. and for a time of 20 to 30 hours.
6. The preparation method according to claim 4, characterized in that: The precipitation reaction is a hydrothermal reaction.
7. The preparation method according to claim 4, characterized in that: The reduction reaction uses a mixed gas of hydrogen and argon as a reducing agent.
8. The preparation method according to claim 7, characterized in that: The volume content of hydrogen in the mixed gas of hydrogen and argon is 5-20%.
9. The preparation method according to claim 4, characterized in that: The reduction reaction is carried out at a temperature of 700 to 1000° C. and for a time of 2 to 6 hours.
10. Use of the hydrotalcite-derived methane cracking catalyst according to any one of claims 1 to 3, characterized in that: The catalyst is used for cracking methane to prepare hydrogen and carbon nanomaterials.
Citation Information
Patent Citations
Preparation method and catalytic application of supported type high-dispersion nickel-based alloy catalyst
CN104368345A
Nickel-gallium alloy catalyst as well as preparation method and application thereof
CN112705208A
Ni-M-coated NiO-Al2O3 catalyst as well as preparation and application thereof
CN115364866A
Ni-based catalysts for combined steam and carbon dioxide reforming with natural gas
KR1020150129566A
Supported high dispersion nickel-based alloy catalyst preparation method and catalytic application thereof
WO2016078261A1