Encapsulated metal-molecular sieve catalyst for N2O decomposition reaction and preparation method of encapsulated metal-molecular sieve catalyst

The packaging metal-molecular sieve catalyst is prepared by coupling the deposition and seed induction method and the packaging metal-molecular sieve catalyst, which solves the problems of high preparation cost and low metal load in the prior art, and realizes efficient catalytic N2O decomposition at lower temperatures, and improves the Stability and impurity resistance of catalysts.

CN118892861APending Publication Date: 2024-11-05SHANXI UNIV +1

Patent Information

Application Number
CN202410952741.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The prior art has problems such as high production cost, low metal loading and poor packaging effect when preparing N2O decomposition catalysts, resulting in poor catalytic performance of the catalyst at high temperatures and is susceptible to impurity gases.

Method used

The encapsulated metal-molecular sieve catalyst is prepared by coupling the deposition and precipitation method with seed induction method, avoiding the use of expensive organic complexing agents, depositing metal species on the surface of the molecular sieve gel by precipitation, and crystallizing in the molecular sieve body phase to form nanometers Or micron-scale transition metal oxide particles improve metal loading and catalyst stability.

Benefits of technology

It realizes efficient catalytic N2O decomposition at lower temperatures, improves the resistance to metal agglomeration and impurity gases of the catalyst, reduces the preparation cost, and the catalyst exhibits excellent catalytic activity and stability within 360-480°C.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892861A_ABST
    Figure CN118892861A_ABST
Patent Text Reader

Abstract

The invention discloses an encapsulated metal-molecular sieve catalyst for N2O decomposition reaction and a preparation method of the encapsulated metal-molecular sieve catalyst, and belongs to the technical field of environmental catalysis. The catalyst is prepared by coupling a deposition-precipitation method and a seed crystal induction method, and specifically comprises the following steps: firstly, directly loading active metal species such as Fe, Co, Ni and Cu on molecular sieve nanocrystals which are not completely grown by adopting the deposition-precipitation method, and then adding the active metal species serving as the seed crystal into silica-alumina gel to induce the growth of a molecular sieve skeleton structure, and centrifuging, washing, drying and roasting to finish the preparation. In the obtained catalyst, active metal species are encapsulated in a molecular sieve bulk phase in the form of nano oxide microcrystals, N2O can be completely catalyzed to be decomposed into N2 and O2 in a medium and low temperature range (360-480 DEG C), and the catalyst has excellent high-temperature agglomeration resistance and impurity gas resistance. The catalyst is simple in preparation process, does not need expensive organic complexing agents, and has industrial application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of environmental catalysis, and in particular relates to an encapsulated metal-molecular sieve catalyst for N2O decomposition reaction and a preparation method thereof. Background Art

[0002] Nitrous oxide (N2O) is one of the six greenhouse gases specified in the Kyoto Protocol. Its single-molecule warming potential is 298 times that of carbon dioxide (CO2), and it has a significant greenhouse effect. N2O emissions occur through two pathways: natural processes and anthropogenic activities. The natural emission process can achieve balance through the nitrogen cycle, while anthropogenic N2O emissions lead to an imbalance in the nitrogen cycle in nature, causing an increase in the concentration of N2O in the atmosphere. Fossil fuel combustion, chemical product production, and agricultural fertilizer use are the main sources of anthropogenic N2O emissions. Controlling and eliminating N2O emissions from motor vehicle exhaust and industrial exhaust such as nitric acid and adipic acid is an important way to alleviate N2O pollution, which is of great significance for the realization of my country's "dual carbon" goals.

[0003] Direct catalytic decomposition of N2O into N2 and O2 is the most ideal N2O emission reduction treatment technology, which has the advantages of simple process, green environmental protection and low cost. However, the NO bond energy in the N2O molecule is as high as 250-270 kJ mol -1 , the direct thermal decomposition temperature exceeds 800℃, and a catalyst needs to be added to the reaction system to promote the breakage of NO bonds and reduce the decomposition temperature. Transition metal oxides represented by spinel Co3O4 are the most widely studied catalysts in this technology. They have excellent activity, are cheap and easy to obtain, and have great potential for industrial application. However, this type of catalyst has a small specific surface area, low utilization of active sites, and is easy to agglomerate at high temperatures. The catalytic performance is significantly affected by impurity gases. In comparison, molecular sieves have rich pore structures, large specific surface areas and stable structures. As carriers encapsulating transition metal oxides, they can be uniformly loaded in the molecular sieve pores and cage structures. The unique micro-nano confined space can effectively inhibit the migration and agglomeration of metal oxide particles in high temperature environments, and has broad application prospects in catalytic N2O decomposition reactions.

[0004] However, currently, encapsulated metal-molecular sieve catalysts are mostly prepared by eutectic crystallization of complex metal salt aqueous solution and molecular sieve gel, and organic ligands are required to bridge metal ions and molecular sieve gel, which has the problems of high preparation cost, low metal loading and poor encapsulation effect. Chinese patent CN 112295594 A discloses an encapsulated metal molecular sieve catalyst and its preparation method and application. The invention uses ethylenediamine, diethylenetriamine and tetraethylenepentamine as ligands, and adopts co-hydrothermal crystallization method to prepare encapsulated metal molecular sieve catalyst, and the mass fraction of metal particles is 0.01-5.0wt%. Chinese patent CN116328827 A discloses the preparation of a metal-loaded molecular sieve and its application as a nitrous oxide decomposition catalyst. The invention first prepares a metal complex solution and a molecular sieve gel, and then fully mixes the two, and prepares metal-loaded CHA and AEI molecular sieve catalysts through crystallization, suction filtration, washing, drying, ammonium exchange, calcination and preactivation. In the preparation process, organic amine, quaternary ammonium base and alkylpiperidinium are selected as metal complexing agents and molecular sieve template agents, and the metal active component loading in the obtained sample is 0.2-5.0wt%. Due to the low loading, the temperature of the catalyst of the invention for completely decomposing N2O exceeds 500°C. Therefore, the development of an encapsulated metal-molecular sieve catalyst with low preparation cost, high active metal loading and excellent N2O decomposition performance is of great value for promoting the development and application of N2O decomposition technology. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide an encapsulated metal-molecular sieve catalyst for N2O decomposition reaction and a preparation method thereof. The present invention prepares the catalyst by coupling the deposition precipitation method + seed induction method. The method can avoid the use of expensive organic complexing agents, can regulate the active metal loading within a wide range, and has the characteristics of low preparation cost and high active metal loading. The obtained catalyst has a transition metal oxide encapsulated in the molecular sieve body phase as an active component, can efficiently catalyze the decomposition of N2O into N2 and O2 within a relatively low temperature range, and has excellent resistance to metal agglomeration and resistance to impurity gases.

[0006] To achieve the above object, the technical solution of the present invention is as follows:

[0007] A method for preparing an encapsulated metal-molecular sieve catalyst for N2O decomposition reaction comprises the following steps:

[0008] Step 1: Mix Si source, Al source, alkali source, deionized water and template agent and stir them thoroughly to obtain molecular sieve gel;

[0009] Step 2: Preliminarily crystallizing part of the molecular sieve gel obtained in step 1 to obtain an incompletely grown molecular sieve nanoparticle suspension;

[0010] Step 3: adding a metal salt aqueous solution dropwise to the suspension obtained in step 2, and stirring sufficiently to allow the metal species to be deposited on the surface of the incompletely grown molecular sieve grains;

[0011] Step 4: Add all the mixture obtained in step 3 dropwise to the remaining molecular sieve gel in step 1, stir thoroughly and then crystallize;

[0012] Step 5: The crystallized product obtained in step 4 is centrifugally washed, dried and calcined to obtain the encapsulated metal-molecular sieve catalyst.

[0013] Furthermore, in step 1, the Si source is one or both of acidic silica sol and tetraethyl orthosilicate; the alkali source is one or both of sodium hydroxide and potassium hydroxide; and the Al source is one or more of aluminum nitrate, aluminum sulfate and sodium aluminate.

[0014] Further, in step 1, the template is one of tetraethylammonium hydroxide, tetraethylammonium bromide, n-butylamine, tetrapropylammonium hydroxide and tetrapropylammonium bromide. According to the type of template, the obtained molecular sieve gel can be divided into MFI type (tetraethylammonium hydroxide or tetraethylammonium bromide), BEA type (tetrapropylammonium hydroxide and tetrapropylammonium bromide) and FAU type (n-butylamine).

[0015] Furthermore, in step 1, the stirring conditions are: 25-45° C., 6-24 h.

[0016] Furthermore, in step 2, the mass of the partial molecular sieve gel accounts for 20-70wt% of the total mass of the molecular sieve gel; the initial crystallization conditions are: 80-120° C., 12-72h.

[0017] Furthermore, in step 3, the metal salt is a nitrate, sulfate or chloride of Fe, Co, Ni or Cu, and the metal ion concentration in the metal salt aqueous solution is 0.01 to 0.5 mol L -1 .

[0018] Furthermore, in step 3, the stirring conditions are: 40-60° C., 3-6 h.

[0019] Furthermore, in step 4, the stirring conditions are: 40-60° C., 6-12 h; and the crystallization conditions are: 100-210° C., 3-72 h.

[0020] Furthermore, in step 5, the drying conditions are: 80-120° C., 6-12 h; and the calcination conditions are: 450-600° C., 4-6 h.

[0021] An encapsulated metal-molecular sieve catalyst prepared by the above-mentioned preparation method, in which active metal Fe, Co, Ni or Cu species are encapsulated in the form of nano-oxide microcrystals in the MFI type, BEA type or FAU type molecular sieve body phase.

[0022] An application of the encapsulated metal-molecular sieve catalyst as described above in the decomposition and removal of N2O.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The present invention adopts a deposition precipitation coupled seed induction method to prepare an encapsulated metal-molecular sieve catalyst, which can avoid the use of expensive complexing agents such as organic amines in the encapsulation step of the prior art, has a low preparation cost, and is more environmentally friendly.

[0025] (2) The method of the present invention has high encapsulation efficiency. The metal oxide particles in the obtained sample can be highly dispersed and evenly distributed in the molecular sieve phase, and the metal species loading can be adjusted within a wide range.

[0026] (3) The catalyst of the present invention has excellent catalytic activity and catalytic stability in the N2O decomposition reaction, can completely catalyze the decomposition of N2O within 360-480°C, is less affected by impurity gases such as O2, NO, H2O, and the structure of the active metal species can remain stable in a high temperature environment. The comprehensive performance of the catalyst is superior to that of metal-molecular sieve catalysts prepared by conventional ion exchange and impregnation methods. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a transmission electron microscopy (TEM) image of the nano molecular sieve catalyst prepared in Example 1;

[0028] Figure 2 This is a transmission electron microscope (TEM) image of the micron molecular sieve catalyst prepared in Example 3;

[0029] Figure 3 This is a graph showing the evaluation results of the N2O catalytic decomposition activity of the catalysts prepared in Examples 1-5 of the present invention;

[0030] Figure 4 This is a graph showing the evaluation results of the N2O catalytic decomposition activity of the catalysts prepared in Example 6 of the present invention and Comparative Example 1. DETAILED DESCRIPTION

[0031] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0032] Example 1

[0033] (1) Weigh 0.02 g of sodium hydroxide (NaOH), 8.91 g of tetrapropylammonium hydroxide aqueous solution (TPAOH, 25 wt%) and 0.73 g of aluminum sulfate 18hydrate (Al2(SO4)3·18H2O) and dissolve them in 40.00 g of deionized water (H2O). Then, add 13.35 g of tetraethyl orthosilicate (TEOS) dropwise using a dropper and stir at room temperature for 24 h to obtain a ZSM-5 molecular sieve gel with SiO2 / Al2O3=57.

[0034] (2) 31.51 g of the ZSM-5 molecular sieve gel prepared in step (1) was placed in a polytetrafluoroethylene hydrothermal crystallization reactor and hydrothermally crystallized at 100° C. for 24 h to obtain an incompletely grown ZSM-5 molecular sieve particle suspension.

[0035] (3) Weigh 1.78 g of cobalt nitrate hexahydrate (Co(NO3)2·6H2O) and dissolve it in 100 mL of deionized water, then add it dropwise into the suspension obtained in step (2), and vigorously stir at 40°C for 3 h to obtain a suspension of ZSM-5 molecular sieve particles containing metallic Co.

[0036] (4) The suspension of ZSM-5 molecular sieve particles containing metal Co obtained in step (3) is added dropwise to the remaining ZSM-5 molecular sieve gel in step (1), and after being fully stirred at 40°C for 6 hours, the mixture is transferred to a polytetrafluoroethylene hydrothermal crystallization reactor and hydrothermally crystallized at 210°C for 3 hours.

[0037] (5) The solid crystallized product is obtained by centrifugation and washed by centrifugation with deionized water until the pH of the centrifuge liquid is 7.

[0038] (6) The wet solid sample after centrifugal washing was placed in a 100°C forced air drying oven for 12 h, and then calcined in a muffle furnace at 550°C for 6 h at a heating rate of 2°C / min. Thus, an encapsulated nano Co-ZSM-5 molecular sieve catalyst with a Co mass fraction of 11 wt% (measured by XRF) was obtained.

[0039] (7) The catalyst was evaluated for N2O decomposition activity under the conditions of 0.1 vol.% N2O / Ar and space velocity GHSV = 10000 h -1 , the reaction temperature is 240~550℃.

[0040] from Figure 1 It can be seen from the electron microscope image that the molecular sieve grain size can reach about 425nm. Figure 3 It can be seen from the N2O decomposition activity evaluation diagram shown that when the reaction temperature is 440°C, the N2O decomposition conversion rate can reach 90%.

[0041] Example 2

[0042] The mass of cobalt nitrate hexahydrate (Co(NO3)2·6H2O) used in step (3) of Example 1 was reduced from 1.78 g to 0.89 g, and the other preparation steps and preparation parameters remained unchanged to obtain an encapsulated nano Co-ZSM-5 molecular sieve catalyst with a Co mass fraction of 5 wt% (measured by XRF). The evaluation was carried out under the same conditions as in Example 1. The evaluation results are as follows: Figure 3 It can be seen that when the reaction temperature is 440°C, the N2O conversion rate increases to 100%.

[0043] Example 3

[0044] The amount of molecular sieve gel used in step (2) of Example 1 was reduced from 31.51 g to 15.75 g, the crystallization time involved in step (4) was extended to 6 h, and the other preparation steps and preparation parameters remained unchanged to obtain an encapsulated micron Co-ZSM-5 molecular sieve catalyst with a Co mass fraction of 11 wt% (measured by XRF). Figure 2 As can be seen from the electron microscope image, the molecular sieve grain size can reach about 1.4 μm. The evaluation was carried out under the same conditions as in Example 1. The evaluation results are shown in FIG. Figure 3 It can be seen that when the reaction temperature is 440°C, the N2O conversion rate is 85%.

[0045] Example 4

[0046] The mass of sodium hydroxide (NaOH) used in step (1) of Example 1 was increased from 0.02g to 0.45g, 8.91g of tetrapropylammonium hydroxide aqueous solution (TPAOH, 25wt%) was changed to 6.2g of tetraethylammonium hydroxide aqueous solution (TEAOH, 35wt%), the crystallization temperature involved in step (4) was reduced from 210°C to 160°C, the time was extended from 3h to 48h, and the other preparation steps and preparation parameters remained unchanged, and an encapsulated Co-β molecular sieve catalyst with a Co mass fraction of 7wt% (measured by XRF) was obtained. The evaluation was carried out under the same conditions as in Example 1, and the evaluation results are as follows: Figure 3 As shown, it can be seen that when the reaction temperature is 440°C, the N2O conversion rate is 73%.

[0047] Example 5

[0048] The 3.56 g of cobalt nitrate hexahydrate (Co(NO3)2·6H2O) used in step (3) of Example 1 was replaced by 1.30 g of nickel nitrate hexahydrate (Ni(NO3)2·6H2O), and the other preparation steps and preparation parameters remained unchanged to obtain an encapsulated nano Ni-ZSM-5 molecular sieve catalyst with a Ni mass fraction of 4 wt% (measured by XRF). The evaluation was carried out under the same conditions as in Example 1. The evaluation results are as follows: Figure 3 It can be seen that when the reaction temperature is 440°C, the N2O conversion rate reaches 70%.

[0049] Example 6

[0050] The catalyst was prepared by the method of Example 2. When evaluating the catalyst performance, 0.1 vol. % NO was mixed into the raw gas of 0.1 vol. % N2O / Ar. The reaction space velocity and reaction temperature were kept the same as those of Example 2. The evaluation results are as follows: Figure 4 It can be seen that the encapsulated nano Co-ZSM-5 molecular sieve catalyst with a Co mass fraction of 5wt% (measured by XRF) has excellent NO resistance, and when the reaction temperature is 440℃, the N2O conversion rate is still close to 100%.

[0051] Comparative Example 1

[0052] (1) Weigh 2 g of commercial Na-type ZSM-5 molecular sieve and set aside.

[0053] (2) Weigh 0.59 g of Co(NO3)2·6H2O and dissolve it in 2 mL of deionized water. Add it dropwise into the ZSM-5 molecular sieve weighed in step (1) while stirring. After the addition is completed, place the sample in a 40°C water bath and let it stand for 6 h.

[0054] (3) The sample after standing was placed in a 100°C forced air drying oven for 12 hours, and then calcined in a muffle furnace at 500°C for 4 hours at a heating rate of 2°C / min. Thus, a Co-ZSM-5 molecular sieve catalyst prepared by the impregnation method was obtained.

[0055] (4) The catalyst was subjected to an evaluation of N2O decomposition activity under the same evaluation conditions as in Example 1.

[0056] from Figure 4 It can be seen from the N2O decomposition activity evaluation diagram shown that when the reaction temperature is 440°C, the N2O decomposition conversion rate is only 63%.

[0057] The above description is only for better explaining the embodiments of the present invention, and is not intended to limit the present invention. Any modification or equivalent substitution that does not depart from the spirit and scope of the present invention shall fall within the scope of the present invention.

Claims

1. A method for preparing an encapsulated metal-molecular sieve catalyst for N2O decomposition reaction, characterized in that: The following steps are involved: Step 1: Mix Si source, Al source, alkali source, deionized water and template agent and stir them thoroughly to obtain molecular sieve gel; Step 2: Preliminarily crystallizing part of the molecular sieve gel obtained in step 1 to obtain an incompletely grown molecular sieve nanoparticle suspension; Step 3: adding a metal salt aqueous solution dropwise to the suspension obtained in step 2, and stirring sufficiently to allow the metal species to be deposited on the surface of the incompletely grown molecular sieve grains; Step 4: Add all the mixture obtained in step 3 dropwise to the remaining molecular sieve gel in step 1, stir thoroughly and then crystallize; Step 5: The crystallized product obtained in step 4 is centrifugally washed, dried and calcined to obtain the encapsulated metal-molecular sieve catalyst.

2. The method for preparing an encapsulated metal-molecular sieve catalyst for N2O decomposition reaction according to claim 1, characterized in that: In step 1, the Si source is one or both of acidic silica sol and tetraethyl orthosilicate; the alkali source is one or both of sodium hydroxide and potassium hydroxide; the Al source is one or more of aluminum nitrate, aluminum sulfate and sodium aluminate; and the template is one of tetraethylammonium hydroxide, tetraethylammonium bromide, n-butylamine, tetrapropylammonium hydroxide and tetrapropylammonium bromide.

3. The method for preparing an encapsulated metal-molecular sieve catalyst for N2O decomposition reaction according to claim 1, characterized in that: In step 1, the stirring conditions are: 25-45° C., 6-24 h.

4. The method for preparing an encapsulated metal-molecular sieve catalyst for N2O decomposition reaction according to claim 1, characterized in that: In step 2, the mass of the partial molecular sieve gel accounts for 20-70wt% of the total mass of the molecular sieve gel; the initial crystallization conditions are: 80-120° C., 12-72h.

5. The method for preparing an encapsulated metal-molecular sieve catalyst for N2O decomposition reaction according to claim 1, characterized in that: In step 3, the metal salt is a nitrate, sulfate or chloride of Fe, Co, Ni or Cu, and the metal ion concentration in the metal salt aqueous solution is 0.01 to 0.5 mol L -1 .

6. The method for preparing an encapsulated metal-molecular sieve catalyst for N2O decomposition reaction according to claim 1, characterized in that: In step 3, the stirring conditions are: 40-60° C., 3-6 h.

7. The method for preparing an encapsulated metal-molecular sieve catalyst for N2O decomposition reaction according to claim 1, characterized in that: In step 4, the stirring conditions are: 40-60° C., 6-12 h; and the crystallization conditions are: 100-210° C., 3-72 h.

8. The method for preparing an encapsulated metal-molecular sieve catalyst for N2O decomposition reaction according to claim 1, characterized in that: In step 5, the drying conditions are: 80-120° C., 6-12 h; and the calcination conditions are: 450-600° C., 4-6 h.

9. An encapsulated metal-molecular sieve catalyst prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The active metal Fe, Co, Ni or Cu species in the catalyst are encapsulated in the MFI type, BEA type or FAU type molecular sieve body phase in the form of nano-oxide microcrystals.

10. Use of the encapsulated metal-molecular sieve catalyst according to claim 9 in the decomposition and removal of N2O.

Citation Information

Patent Citations

  • Method for synthesizing metal-ZSM molecular sieve

    CN106276963A

  • Methanol-to-propylene nano stacked ZSM-5 molecular sieve preparation method

    CN109126861A

  • Bifunctional catalyst of sodium-free silicon-aluminum molecular sieve for encapsulating metal nanoparticles and preparation method of bifunctional catalyst

    CN109731608A

  • Copper-based CHA type aluminosilicate molecular sieve catalyst and preparation method thereof

    CN112473730A

  • Zeolite molecular sieve supported metal catalyst as well as synthesis method and application thereof

    CN113649064A

Cited By

  • Encapsulated composite catalyst and application thereof in preparation of low-carbon olefin by oxidative cracking of naphtha

    CN119425777A