Fine silt dispersing agent as well as preparation method and application thereof
Patent Information
- Application Number
- CN202410931855.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-12
AI Technical Summary
优点是分散效果好、分散稳定性高,但缺点是制备成本较高;表面活性剂,如十二烷基硫酸钠、十二烷基苯磺酸钠等,优点是制备成本低廉且分散效果较好,但缺点是有些表面活性剂在一些情况下可能会影响锂云母精矿的品质;碱性分散剂,如氢氧化钠、氢氧化钾、石灰等,优点是操作简单且在一定程度上有抑泡作用,但缺点是分散效果可能不如有机分散剂
[0019] The fine mud dispersant provided by the invention realizes flotation separation of highly weathered lepidolite ore under less desliming conditions. The fine mud dispersant has good dispersion effect, low manufacturing cost and will not affect the grade of the concentrate.
Smart Images

Figure BDA0004939924680000031 
Figure BDA0004939924680000041 
Figure BDA0004939924680000051
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of mineral flotation, and in particular to a fine mud dispersant and a preparation method and application thereof. Background Art
[0002] As an important lithium mineral, lepidolite plays a key role in the extraction and utilization of lithium resources. It is widely used in lithium-ion batteries, glass ceramics, ceramic materials, fireproof materials and other fields. With the vigorous development of the new energy industry, especially the popularity of electric vehicles and energy storage equipment, the demand for lithium resources continues to increase, thus promoting the development and utilization of lepidolite.
[0003] Existing lithium mica flotation fine mud dispersants mainly include organic polymer dispersants, such as polyacrylamide (PAM), polyvinyl alcohol (PVA), etc. The advantages are good dispersion effect and high dispersion stability, but the disadvantage is high preparation cost; surfactants, such as sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, etc., have the advantages of low preparation cost and good dispersion effect, but the disadvantage is that some surfactants may affect the quality of lithium mica concentrate in some cases; alkaline dispersants, such as sodium hydroxide, potassium hydroxide, lime, etc., have the advantages of simple operation and anti-foaming effect to a certain extent, but the disadvantage is that the dispersion effect may not be as good as organic dispersants. Therefore, in recent years, highly dispersible and selective lithium mica flotation fine mud dispersants have gradually become a research hotspot. Developing a fine mud dispersant to achieve efficient separation of lithium mica flotation under less desludging conditions is of great significance to improving the separation index of strongly weathered lithium mica ore in Yichun area. Summary of the invention
[0004] Based on the technical problems existing in the background technology, the present invention proposes a fine mud dispersant and a preparation method and application thereof.
[0005] The invention provides a fine mud dispersant, which comprises the following raw materials in parts by weight: 5-6 parts of a surfactant, 2-3 parts of an organic polymer dispersant, and 0.5-1 part of an alkaline dispersant.
[0006] The fine mud dispersant of the present invention cannot achieve the optimal dispersion effect on the fine mud if a surfactant, an organic polymer dispersant or an alkaline dispersant is added alone. The surfactant, the organic polymer dispersant and the alkaline dispersant are used in combination to prevent the aggregation and precipitation of the fine mud particles and maintain the dispersed state.
[0007] Preferably, the surfactant is selected from one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate and sodium octanoate.
[0008] Surfactants can reduce the surface tension of the liquid in the liquid phase, thereby reducing the interaction force between fine mud particles and slowing down the agglomeration rate of the particles.
[0009] Preferably, the organic polymer dispersant is selected from one or more of polyacrylamide, polyether and polyvinyl pyrrolidone.
[0010] The polymer chains formed by organic polymer dispersant molecules in water have a certain hydrophilicity and can be adsorbed on the surface of fine mud to form a dispersion layer, so that the surface of fine mud has a certain charge, generating electrostatic repulsion, preventing the coagulation and aggregation between fine muds, and maintaining the dispersed state of particles. In addition, the molecular structure of organic polymer dispersants contains hydrophilic groups and hydrophobic groups, forming physical or chemical adsorption between the water phase and the solid phase (lepidolite surface), thereby changing the properties of the particle surface; this adsorption can reduce the adhesion ability of the particle surface, weaken the interaction between particles, and thus prevent the aggregation and precipitation of particles, and maintain the dispersed state of particles.
[0011] Preferably, the alkaline dispersant is selected from one or more of sodium hydroxide and lime.
[0012] The alkaline dispersant allows the fine mud to be fully dispersed during the flotation separation of lepidolite, preventing the fine mud from covering the surface of the lepidolite.
[0013] The present invention also provides a method for preparing a fine mud dispersant, comprising the following steps: uniformly mixing a surfactant, an organic polymer dispersant and an alkaline dispersant to obtain the fine mud dispersant.
[0014] Preferably, the preparation of the fine mud dispersant aqueous solution comprises dissolving the fine mud dispersant in water to obtain the fine mud dispersant aqueous solution.
[0015] More preferably, the mass fraction of the fine mud dispersant aqueous solution is 3-10wt%.
[0016] The preparation method proposed by the invention is simple, has low manufacturing cost and the obtained fine mud dispersant will not affect the grade of concentrate; the mass fraction of the fine mud dispersant aqueous solution is within a suitable range, which can prevent the coagulation and aggregation of fine muds and maintain the dispersed state of particles.
[0017] The present invention also proposes the use of the above-mentioned fine mud dispersant or the fine mud dispersant prepared by the above-mentioned preparation method in the flotation separation of lepidolite ore.
[0018] The beneficial effects of the present invention are:
[0019] The fine mud dispersant provided by the invention realizes the flotation separation of highly weathered lepidolite ore under the condition of less desludging, and the fine mud dispersant has good dispersing effect, low manufacturing cost and will not affect the grade of concentrate. DETAILED DESCRIPTION
[0020] The technical solution of the present invention is described in detail through specific embodiments.
[0021] Unless otherwise specified, the materials, reagents, etc. used in the following examples and comparative examples can be obtained from commercial sources.
[0022] Example 1
[0023] A method for preparing a fine mud dispersant comprises the following steps: uniformly mixing 25g of sodium dodecylbenzene sulfonate, 10g of sodium octoate, 13.5g of polyvinyl pyrrolidone and 1.5g of sodium hydroxide to obtain a fine mud dispersant; and dissolving the fine mud dispersant in water to obtain a 5wt% fine mud dispersant aqueous solution.
[0024] Taking a lithium mica mine in Yifeng as the ore sample, its chemical composition is shown in Table 1:
[0025] Table 1
[0026]
[0027] The flotation collector is coconut amine. The collector and fine mud dispersant are used to carry out coarse and fine flotation of the ore sample. The flotation process conditions are as follows:
[0028] (1) Ore sample pretreatment: The ore samples were screened to make the floating particle size less than -0.074 mm account for 24%, and the -400 mesh fine-grained ore mud in some ore samples was removed, and the desludging amount was 3%;
[0029] (2) Positive flotation enrichment: Add 400g of ore sample to a 1L flotation tank, add 750mL of tap water to make a slurry, stir thoroughly, add 200g / t of fine mud dispersant aqueous solution and stir for 3min; then add 320g / t of coconut amine and stir for 4min. Aeration flotation, the obtained foam product is the lepidolite rough concentrate, and the product in the flotation tank is the flotation tailings; the obtained lepidolite rough concentrate is slurried with tap water, and the foam product obtained after primary selection is the lepidolite concentrate, and the product in the flotation tank is the lepidolite middlings.
[0030] Through the prepared fine mud dispersant and the one-coarse-one-fine direct flotation process conditions, a lithium mica concentrate with a Li2O grade and a recovery rate of 2.08% and 84.35% was finally obtained, and the separation index was good.
[0031] Example 2
[0032] A method for preparing a fine mud dispersant comprises the following steps: uniformly mixing 25g of sodium dodecylbenzene sulfonate, 10g of sodium octoate, 14g of polyvinyl pyrrolidone and 1g of sodium hydroxide to obtain a fine mud dispersant; and dissolving the fine mud dispersant in water to obtain a 5wt% fine mud dispersant aqueous solution.
[0033] The tailings of a tantalum-niobium ore in Yichun after pre-enrichment of tantalum and niobium by gravity separation were taken as the ore sample, and its chemical composition is shown in Table 2:
[0034] Table 2
[0035]
[0036] The flotation collector is coconut amine. This collector and fine mud dispersant are used to carry out coarse and fine flotation of the ore sample. The flotation process conditions are as follows:
[0037] (1) Ore sample pretreatment: Screen the ore samples to make the floating particle size less than -0.074 mm account for 25%, remove the -400 mesh fine-grained sludge in some ore samples, and the desludge amount is 4%;
[0038] (2) Positive flotation enrichment: Add 420g of ore sample to a 1L flotation tank, add 740mL of tap water to make a slurry, stir thoroughly, add 180g / t of the above-mentioned fine mud dispersant aqueous solution and stir for 3min; then add 350g / t of coconut amine and stir for 4min. Aeration flotation, the obtained foam product is the lepidolite rough concentrate, and the product in the flotation tank is the flotation tailings; the obtained lepidolite rough concentrate is slurried with tap water, and the foam product obtained after primary selection is the lepidolite concentrate, and the product in the flotation tank is the lepidolite middlings.
[0039] By using the prepared fine mud dispersant and its one-coarse-one-fine direct flotation process conditions, a lithium mica concentrate with a Li2O grade and a recovery rate of 2.39% and 86.01% was finally obtained, and the separation index was good.
[0040] Comparative Example 1
[0041] A method for preparing a fine mud dispersant comprises the following steps: uniformly mixing 35g of sodium octoate and 15g of polyether to obtain a fine mud dispersant; and dissolving the fine mud dispersant in water to obtain a 5wt% fine mud dispersant aqueous solution.
[0042] Taking a lithium mica mine in Yifeng as the ore sample, its chemical composition is shown in Table 1:
[0043] Table 1
[0044]
[0045] The flotation collector is coconut amine. The collector and fine mud dispersant are used to carry out coarse and fine flotation of the ore sample. The flotation process conditions are as follows:
[0046] (1) Ore sample pretreatment: The ore samples were screened to make the floating particle size less than -0.074 mm account for 24%, and the -400 mesh fine-grained ore mud in some ore samples was removed, and the desludging amount was 3%;
[0047] (2) Positive flotation enrichment: Add 400g of ore sample to a 1L flotation tank, add 750mL of tap water to make a slurry, stir thoroughly, add 200g / t of the above-mentioned fine mud dispersant aqueous solution and stir for 3min; then add 320g / t of coconut amine and stir for 4min. Aeration flotation, the obtained foam product is the lepidolite rough concentrate, and the product in the flotation tank is the flotation tailings; the obtained lepidolite rough concentrate is slurried with tap water, and the foam product obtained after primary selection is the lepidolite concentrate, and the product in the flotation tank is the lepidolite middlings.
[0048] Through the prepared fine mud dispersant and the one-coarse-one-fine positive flotation process conditions, a lithium mica concentrate with a Li2O grade and a recovery rate of 1.65% and 70.26% was finally obtained, and the separation index was poor.
[0049] Comparative Example 2
[0050] A method for preparing a fine mud dispersant comprises the following steps: uniformly mixing 40g of sodium dodecylbenzene sulfonate and 10g of polyvinyl pyrrolidone to obtain a fine mud dispersant; and dissolving the fine mud dispersant in water to obtain a 5wt% fine mud dispersant aqueous solution.
[0051] Taking a lithium mica mine in Yifeng as the ore sample, its chemical composition is shown in Table 1:
[0052] Table 1
[0053]
[0054] The flotation collector is coconut amine. The collector and fine mud dispersant are used to carry out coarse and fine flotation of the ore sample. The flotation process conditions are as follows:
[0055] (1) Ore sample pretreatment: The ore samples were screened to make the floating particle size less than -0.074 mm account for 24%, and the -400 mesh fine-grained ore mud in some ore samples was removed, and the desludging amount was 3%;
[0056] (2) Positive flotation enrichment: Add 400g of ore sample to a 1L flotation tank, add 750mL of tap water to make a slurry, stir thoroughly, add 200g / t of the above-mentioned fine mud dispersant aqueous solution and stir for 3min; then add 320g / t of coconut amine and stir for 4min. Aeration flotation, the obtained foam product is the lepidolite rough concentrate, and the product in the flotation tank is the flotation tailings; the obtained lepidolite rough concentrate is slurried with tap water, and the foam product obtained after primary selection is the lepidolite concentrate, and the product in the flotation tank is the lepidolite middlings.
[0057] Through the prepared fine mud dispersant and its one-coarse-one-fine positive flotation process conditions, a lithium mica concentrate with a Li2O grade and a recovery rate of 1.79% and 76.21% was finally obtained, and the separation index was general.
[0058] In summary, the application of the fine mud dispersant provided by the present invention in the flotation separation of lepidolite ore makes the flotation separation index of the lepidolite ore better.
[0059] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A fine mud dispersant, characterized in that: The invention comprises the following raw materials in parts by weight: 5-6 parts of surfactant, 2-3 parts of organic polymer dispersant and 0.5-1 part of alkaline dispersant.
2. The fine mud dispersant according to claim 1, characterized in that: The surfactant is selected from one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate and sodium octanoate.
3. The fine mud dispersant according to claim 1, characterized in that: The organic polymer dispersant is selected from one or more of polyacrylamide, polyether and polyvinyl pyrrolidone.
4. The fine mud dispersant according to claim 1, characterized in that: The alkaline dispersant is selected from one or more of sodium hydroxide and lime.
5. A method for preparing the fine mud dispersant according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: uniformly mixing a surfactant, an organic polymer dispersant and an alkaline dispersant to obtain a fine mud dispersant.
6. The preparation method according to claim 5, characterized in that: The preparation of the fine mud dispersant aqueous solution comprises dissolving the fine mud dispersant in water to obtain the fine mud dispersant aqueous solution.
7. The preparation method according to claim 6, characterized in that: The mass fraction of the fine mud dispersant aqueous solution is 3-10wt%.
8. Use of the fine mud dispersant according to any one of claims 1 to 4 or the fine mud dispersant prepared by the preparation method according to any one of claims 5 to 7 in the flotation separation of lepidolite ore.
Citation Information
Patent Citations
Flotation separation method for aedelforsite and quartz
CN103691563A
Beneficiation method of micro-fine particle zinc oxide ore
CN106540815A
Energy-saving, environmental-friendly, clean and high-efficient compound floatation agent
CN108435430A
Lepidolite ore beneficiation method based on hyperdispersant
CN115957892A
Method for efficiently recovering micro-fine particle slime
CN116273435A