Production process of diaphragm valve

By mixing pig iron, scrap steel and stainless steel and melting it in a forging furnace, adding borax to remove impurities, and performing three calcining and secondary forging, combining water-cooled molding and fine processing, the existing diaphragm valve production process is solved inefficient and structure. The problem of insufficient strength achieves higher mechanical properties and durability.

CN118893424APending Publication Date: 2024-11-05KUNSHAN LION HYGIENIC MATERIALS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410939494.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The production process of existing diaphragm valves is low and the steps are cumbersome, resulting in insufficient strength and service life of the valve body, and non-integrated casting molding.

Method used

It uses metal materials such as pig iron, scrap steel, stainless steel, etc., and then melts it in a forging furnace. Add borax to remove impurities. It undergoes three calcination and secondary forging, combined with water-cooled molding and fine processing, and finally undergoes anti-rust treatment.

Benefits of technology

Simplify production steps, improve the structural strength and mechanical properties of the valve body, enhance high temperature and corrosion resistance, and extend service life.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A production process of a diaphragm valve belongs to the technical field of diaphragm valve production and comprises the following steps: S1, selecting raw materials of the diaphragm valve, including one or a mixture of more of metal materials such as pig iron, scrap steel, stainless steel and scrap iron; s2, the raw materials in the S1 are smashed, so that the raw materials are more conveniently put into a container used for melting, meanwhile, the melting speed is increased, and energy generated in the melting process and energy waste are reduced; and S3, the raw materials are put into a forging furnace to be melted into molten metal, borax is added in the melting process, impurities contained in the raw materials are removed through the borax, the molten metal is purer, and therefore the structural strength of the diaphragm valve formed subsequently is improved. According to the production process of the diaphragm valve, impurities of the valve body are greatly reduced through three times of calcination treatment, so that the diaphragm valve is more durable, the high temperature resistance and the corrosion resistance of the diaphragm valve are improved, and the overall advantages of the valve body are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of diaphragm valve production, in particular to a production process of a diaphragm valve. Background Art

[0002] The diaphragm valve is suitable for use in pipelines of various concentrations of aqua regia, sulfuric acid, hydrochloric acid, hydrofluoric acid and various organic acids, strong acids, and strong oxidants at -50 to 150°C. It is also suitable for use in pipelines of various concentrations of strong alkali organic solvents and other corrosive gases and liquid media.

[0003] At present, in the diaphragm valve manufacturing industry, domestic spherical diaphragm valve bodies are all made of ordinary high-speed steel materials, or stainless steel materials are machined into spherical diaphragm valve bodies. This manufacturing method is not only inefficient, but also has complicated production steps. The valve body needs to be finely polished during the production process. At the same time, the valve body is not cast in one piece, which reduces its service life and mechanical strength. Summary of the invention

[0004] The present invention mainly solves the technical problems existing in the above-mentioned prior art and provides a production process for a diaphragm valve.

[0005] The above technical problem of the present invention is mainly solved by the following technical solution: A production process of a diaphragm valve comprises the following steps:

[0006] S1. Select the raw materials of the diaphragm valve, including one or more mixed metal materials such as pig iron, scrap steel, stainless steel, iron filings, etc.;

[0007] S2, crushing the raw materials in S1 to make it easier to put them into the container used for melting, while increasing the melting speed and reducing the energy and energy waste generated during the melting process;

[0008] S3, putting the raw materials into a forging furnace for melting, melting them into molten metal, and adding borax during the melting process, so as to remove impurities contained in the raw materials through borax, making the molten liquid purer, thereby improving the structural strength of the subsequent diaphragm valve after molding;

[0009] S4, pouring the obtained molten metal into a prefabricated mold and cooling it to form;

[0010] Among them, cooling can be natural cooling or water cooling. Water cooling can increase the cooling speed after forming, thereby speeding up the production progress;

[0011] S5. The formed metal parts are subjected to secondary forging treatment. The secondary forging treatment is divided into three steps. The first step is to place the metal parts in a forging furnace for calcination at a temperature of 600-700°C for 1.5-2h, and cool them to 100°C after the calcination is completed. The second step is to place the metal parts in a forging furnace for secondary calcination on the basis of the first step. The calcination temperature is 700-800°C for 1.5-2h, and after the calcination is completed, it is cooled to 100°C for the third calcination. The third calcination temperature is 800-900°C for 0.5-1h, and it is cooled naturally.

[0012] By calcining the metal parts three times, the internal structure of the diaphragm valve assembly is made tighter and more reliable, and the presence of impurities is reduced, thereby improving its subsequent mechanical properties and increasing its service life;

[0013] S6. After the metal parts are calcined, they are finely processed. The surface and internal burrs can be polished and cleaned by grinding equipment, so that they will be smoother during subsequent use;

[0014] S7, performing anti-rust treatment on the metal parts obtained above, wherein the anti-rust treatment step includes soaking the metal parts with anti-rust oil or coating the metal parts with anti-rust liquid to achieve anti-rust operation on the valve body, so that the valve body will not be affected by air humidity and will not rust during storage;

[0015] S8. Assemble the metal parts obtained in the above steps to form a diaphragm valve, and package and store it.

[0016] Preferably, after the raw materials are selected as described in S1, they can be cleaned to reduce impurities or rust on their surfaces, thereby ensuring that the stability of the raw materials will not be affected by impurities during subsequent processing.

[0017] Preferably, the temperature of the forging furnace in S2 is 1400-1600° C., and the melting time is 1-2 h.

[0018] Preferably, the shape of the prefabricated mold in S4 may be the shape of each metal component used in the diaphragm valve.

[0019] Preferably, the grinding equipment in S6 can be used with a grinder or by sandblasting.

[0020] Preferably, the cooling in S4 can be natural cooling or water cooling. Water cooling can increase the cooling speed after molding, thereby speeding up the production progress.

[0021] Compared with the prior art, the present invention provides a production process for a diaphragm valve, which has the following beneficial effects:

[0022] 1. The production process of the diaphragm valve is simple and convenient. The valve body and valve body components are cast and formed at the same time, which improves the overall structural strength and mechanical strength of the valve body and makes it less prone to fracture and wear. At the same time, the three-time calcination treatment greatly reduces the impurities in the valve body, making it more durable and improving its high temperature resistance and corrosion resistance, thereby enhancing the overall advantages of the valve body.

[0023] 2. The production process of the diaphragm valve uses borax to remove impurities contained in the raw materials, making the melt purer, thereby improving the structural strength of the subsequent diaphragm valve after molding. DETAILED DESCRIPTION

[0024] Embodiment 1:

[0025] A production process for a diaphragm valve comprises the following steps:

[0026] S1. Select the raw materials of the diaphragm valve, including one or more mixed metal materials such as pig iron, scrap steel, stainless steel, iron filings, etc.;

[0027] Among them, after the raw materials are selected, they can be cleaned to reduce impurities or rust on their surface, thereby ensuring that the stability of the raw materials will not be affected by impurities in subsequent processing;

[0028] S2, crushing the raw materials in S1 to make it easier to put them into the container used for melting, while increasing the melting speed and reducing the energy and energy waste generated during the melting process;

[0029] S3, putting the raw materials into a forging furnace for melting, melting them into molten metal, and adding borax during the melting process, so as to remove impurities contained in the raw materials through borax, making the molten liquid purer, thereby improving the structural strength of the subsequent diaphragm valve after molding;

[0030] The forging furnace temperature is 1400-1600℃, and the melting time is 1-2h;

[0031] S4, pouring the obtained molten metal into a prefabricated mold and cooling it to form;

[0032] The shape of the prefabricated mold can be the shape of each metal part used in the diaphragm valve;

[0033] S5. The formed metal parts are subjected to secondary forging treatment. The secondary forging treatment is divided into three steps. The first step is to place the metal parts in a forging furnace for calcination at a temperature of 600-700°C for 1.5-2h, and cool them to 100°C after the calcination is completed. The second step is to place the metal parts in a forging furnace for secondary calcination on the basis of the first step. The calcination temperature is 700-800°C for 1.5-2h, and after the calcination is completed, it is cooled to 100°C for the third calcination. The third calcination temperature is 800-900°C for 0.5-1h, and it is cooled naturally.

[0034] By calcining the metal parts three times, the internal structure of the diaphragm valve assembly is made tighter and more reliable, and the presence of impurities is reduced, thereby improving its subsequent mechanical properties and increasing its service life;

[0035] S6. After the metal parts are calcined, they are finely processed. The surface and internal burrs can be polished and cleaned by grinding equipment, so that they will be smoother during subsequent use;

[0036] S7, performing anti-rust treatment on the metal parts obtained above, wherein the anti-rust treatment step includes soaking the metal parts with anti-rust oil or coating the metal parts with anti-rust liquid to achieve anti-rust operation on the valve body, so that the valve body will not be affected by air humidity and will not rust during storage;

[0037] S8. Assemble the metal parts obtained in the above steps to form a diaphragm valve, and package and store it.

[0038] The diaphragm valve obtained through the above steps has simple and convenient production steps. The valve body and valve body components are cast and formed at the same time, which improves the overall structural strength and mechanical strength of the valve body and makes it less prone to fracture and wear. At the same time, the three calcination treatments greatly reduce the impurities in the valve body, making it more durable and improving its high temperature resistance and corrosion resistance, thereby enhancing the overall advantages of the valve body.

[0039] Embodiment 2:

[0040] A production process for a diaphragm valve comprises the following steps:

[0041] S1. Select the raw materials of the diaphragm valve, including one or a mixture of pig iron, scrap steel, and stainless steel metal materials;

[0042] Among them, after the raw materials are selected, they can be cleaned to reduce impurities or rust on their surface, thereby ensuring that the stability of the raw materials will not be affected by impurities in subsequent processing;

[0043] S2, crushing the raw materials in S1 to make it easier to put them into the container used for melting, while increasing the melting speed and reducing the energy and energy waste generated during the melting process;

[0044] S3, putting the raw materials into a forging furnace for melting, melting them into molten metal, and adding borax during the melting process, so as to remove impurities contained in the raw materials through borax, making the molten liquid purer, thereby improving the structural strength of the subsequent diaphragm valve after molding;

[0045] The forging furnace temperature is 1500°C and the melting time is 1.5h;

[0046] S4, pouring the obtained molten metal into a prefabricated mold and cooling it to form;

[0047] The shape of the prefabricated mold can be the shape of each metal part used in the diaphragm valve;

[0048] S5. The formed metal parts are subjected to secondary forging treatment. The secondary forging treatment is divided into three steps. The first step is to place the metal parts in a forging furnace for calcination at a temperature of 600°C for 1.5 hours, and cool them to 100°C after the calcination is completed. The second step is to place the metal parts in a forging furnace for secondary calcination based on the first step. The calcination temperature is 800°C for 1 hour, and after the calcination is completed, cool them to 100°C for the third calcination. The third calcination temperature is 900°C for 0.5 hours, and allow them to cool naturally.

[0049] By calcining the metal parts three times, the internal structure of the diaphragm valve assembly is made tighter and more reliable, and the presence of impurities is reduced, thereby improving its subsequent mechanical properties and increasing its service life;

[0050] S6. After the metal parts are calcined, they are finely processed. The surface and internal burrs can be polished and cleaned by grinding equipment, so that they will be smoother during subsequent use;

[0051] S7, performing anti-rust treatment on the metal parts obtained above, wherein the anti-rust treatment step includes soaking the metal parts with anti-rust oil or coating the metal parts with anti-rust liquid to achieve anti-rust operation on the valve body, so that the valve body will not be affected by air humidity and will not rust during storage;

[0052] S8. Assemble the metal parts obtained in the above steps to form a diaphragm valve, and package and store it.

[0053] Finally, it should be pointed out that the above embodiments are only representative examples of the present invention. Obviously, the present invention is not limited to the above embodiments, and there are many variations. Any simple modification, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention should be considered to belong to the protection scope of the present invention.

Claims

1. A production process for a diaphragm valve, comprising the following steps: S1. Select the raw materials of the diaphragm valve, including one or more mixed metal materials such as pig iron, scrap steel, stainless steel, iron filings, etc.; S2, crushing the raw materials in S1 to make it easier to put them into the container used for melting, while increasing the melting speed and reducing the energy and energy waste generated during the melting process; S3, putting the raw materials into a forging furnace for melting, melting them into molten metal, and adding borax during the melting process, so as to remove impurities contained in the raw materials through borax, making the molten liquid purer, thereby improving the structural strength of the subsequent diaphragm valve after molding; S4, pouring the obtained molten metal into a prefabricated mold and cooling it to form; Among them, cooling can be natural cooling or water cooling. Water cooling can increase the cooling speed after forming, thereby speeding up the production progress; S5. The formed metal parts are subjected to secondary forging treatment. The secondary forging treatment is divided into three steps. The first step is to place the metal parts in a forging furnace for calcination at a temperature of 600-700°C for 1.5-2h, and cool them to 100°C after the calcination is completed. The second step is to place the metal parts in a forging furnace for secondary calcination on the basis of the first step. The calcination temperature is 700-800°C for 1.5-2h, and after the calcination is completed, it is cooled to 100°C for the third calcination. The third calcination temperature is 800-900°C for 0.5-1h, and it is cooled naturally. By calcining the metal parts three times, the internal structure of the diaphragm valve assembly is made tighter and more reliable, and the presence of impurities is reduced, thereby improving its subsequent mechanical properties and increasing its service life; S6. After the metal parts are calcined, they are finely processed. The surface and internal burrs can be polished and cleaned by grinding equipment, so that they will be smoother during subsequent use; S7, performing anti-rust treatment on the metal parts obtained above, wherein the anti-rust treatment step includes soaking the metal parts with anti-rust oil or coating the metal parts with anti-rust liquid to achieve anti-rust operation on the valve body, so that the valve body will not be affected by air humidity and will not rust during storage; S8. Assemble the metal parts obtained in the above steps to form a diaphragm valve, and package and store it.

2. The production process of a diaphragm valve according to claim 1, characterized in that: As described in S1, after the raw materials are selected, they can be cleaned to reduce impurities or rust on their surfaces, thereby ensuring that the stability of the raw materials will not be affected by impurities during subsequent processing.

3. The production process of a diaphragm valve according to claim 1, characterized in that: The temperature of the forging furnace in S2 is 1400-1600°C, and the melting time is 1-2h.

4. The production process of a diaphragm valve according to claim 1, characterized in that: The shape of the prefabricated mold in S4 may be the shape of each metal component used in the diaphragm valve.

5. The production process of a diaphragm valve according to claim 1, characterized in that: The grinding equipment in S6 can be a grinder or sandblasting.

6. The production process of a diaphragm valve according to claim 1, characterized in that: The cooling described in S4 can be natural cooling or water cooling. Water cooling can increase the cooling speed after molding, thereby speeding up the production progress.

Citation Information

Patent Citations

  • Preparation method for diaphragm valve body through cast molding

    CN102994889A

  • Preparation method of 4N tellurium

    CN109319744A

  • Production technology for cast steel valve

    CN109680222A

  • Rail transit derailment valve casting process

    CN111230070A

  • CASTED Fe-Cr-X ELBOW PIPE AND MANUFACTURING METHODTHEREOF