Preparation method of sulfur, nitrogen and boron co-doped lithium iron phosphate
Through the preparation method of lithium iron phosphate co-doped sulfur, nitrogen and boron, biomass carbon and boron doped carbon nanotubes are used to form a conductive electronic layer and a three-dimensional conductive network, which solves the conductive properties and lithium ion diffusion of lithium iron phosphate materials. Improved high-rate performance and cycle stability.
Patent Information
- Application Number
- CN202410846805.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-06-27
AI Technical Summary
The prior art cannot effectively improve the electronic conductivity and lithium ion diffusion rate of lithium iron phosphate cathode materials, resulting in the problem of structural collapse and short cycle life under large-scale discharge conditions.
Using the preparation method of lithium iron phosphate co-doped with sulfur, nitrogen and boron, boron is used to prepare boron-doped carbon nanotubes by activating the biomass carbon, and mixing it with iron, phosphorus, lithium and sulfur sources to perform the Ball milling, spray drying and high-temperature sintering form lithium iron phosphate co-doped with sulfur, nitrogen and boron, forming a continuous conductive electronic layer and a three-dimensional conductive network structure.
It improves the electrochemical performance of lithium iron phosphate, especially the maximum rate performance and cycle stability, reduces impedance, and extends the cycle life of lithium-ion batteries.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion battery positive electrode materials, and in particular to a method for preparing sulfur, nitrogen and boron co-doped lithium iron phosphate. Background Art
[0002] Lithium iron phosphate has the advantages of high theoretical specific capacity (170mAh / g), low cost, and environmental friendliness, and is widely used in electric vehicles and energy storage; however, its inherent low electronic conductivity and lithium ion diffusion rate limit its further development. In order to solve this problem, the main methods currently used are carbon coating, metal and non-metal doping, and particle nano-sizing. Non-metallic doping is one of the ways to improve the intrinsic conductivity of lithium iron phosphate. The non-metallic doping elements commonly used by researchers are nitrogen, phosphorus, sulfur, and boron. Different metal element doping has different effects on the performance of lithium iron phosphate. Therefore, researchers often use multi-element doping to modify lithium iron phosphate.
[0003] Existing technical methods usually use traditional carbon materials such as sucrose, glucose, and crystal sugar as carbon sources to coat lithium iron phosphate positive electrode materials. Although this method improves the electronic conductivity of the lithium iron phosphate positive electrode material to a certain extent, the above-mentioned coating method has limitations on the control of lithium iron phosphate particle size, electronic conductivity, and lithium ion diffusion and transport. It is easy to cause the structure of the lithium iron phosphate positive electrode material to collapse under high-rate discharge conditions, which in turn causes the lithium-ion battery prepared using the lithium iron phosphate positive electrode material to face the problem of short cycle life.
[0004] For example, the patent with publication number CN107359336A discloses a method for preparing lithium iron phosphate, comprising the following steps: a) mixing an iron source, a phosphorus source, a lithium source and a carbon source uniformly, and calcining them under a protective atmosphere to obtain a calcined product; b) grinding the calcined product and drying it; c) calcining the dried calcined product again under a protective atmosphere to obtain lithium iron phosphate. Another patent with publication number CN108493424A discloses a nitrogen, phosphorus and sulfur co-doped composite carbon material, a preparation method thereof and a lithium ion battery, the method comprising: 1) mixing a nitrogen-containing biomass carbon material, a phosphorus-doped graphene precursor, a sulfur source and an activator, impregnating them with water, and then drying them; 2) then activating them at 600°C to 1000°C to obtain a nitrogen, phosphorus and sulfur co-doped composite carbon material.
[0005] However, the carbon source coating method adopted in the above patents cannot fundamentally solve the problems of poor electronic conductivity and lithium ion diffusion of lithium iron phosphate positive electrode materials. It has limitations on the regulation of lithium iron phosphate particle size, electronic conductivity and lithium ion diffusion and transport, and cannot further improve the rate performance of lithium iron phosphate positive electrode materials. Summary of the invention
[0006] The present invention provides a method for preparing lithium iron phosphate co-doped with sulfur, nitrogen and boron, so as to solve the technical problem that the existing method for preparing element-doped lithium iron phosphate positive electrode materials has limitations on the regulation of lithium iron phosphate particle size, electronic conductivity and lithium ion diffusion and transport, and cannot further improve the rate performance of lithium iron phosphate positive electrode materials.
[0007] The embodiments of the present invention are implemented by the following technical solutions:
[0008] A method for preparing sulfur, nitrogen and boron co-doped lithium iron phosphate comprises the following steps:
[0009] S1: Activate the biochar;
[0010] S2: Preparation of boron-doped carbon nanotubes;
[0011] S3: mixing the activated biomass carbon, boron-doped carbon nanotubes, iron source, phosphorus source, lithium source and sulfur source to obtain a suspension;
[0012] S4: ball-milling, spray-drying and high-temperature sintering the suspension to obtain sulfur-, nitrogen- and boron-coated lithium iron phosphate.
[0013] The present technical solution uses cheap biochar as raw material, which reduces the raw material cost and production cost. At the same time, the biochar itself has nitrogen source and carbon source, which saves the cost of adding nitrogen source separately. The nitrogen source and carbon source will form a continuous conductive electron layer after high-temperature sintering, providing a channel for lithium ion insertion and extraction, thereby improving its electrical performance.
[0014] The present invention simultaneously grafts boron onto carbon nanotubes, which can make boron doping in lithium iron phosphate more uniform; in addition, the addition of carbon nanotubes can increase the conductivity of lithium iron phosphate, and further increase the electrochemical performance of lithium iron phosphate, especially the high rate performance;
[0015] The addition of nitrogen, sulfur and boron can make the carbon coating on the surface of lithium iron phosphate more uniform, further improving the electrical properties of lithium iron phosphate.
[0016] Preferably, in the step S1, phosphoric acid is added to the biochar for activation treatment.
[0017] By adopting this technical solution, nitrogen-containing biochar such as plant straw, dead bark, and peanut shells are used as nitrogen and carbon sources, and phosphoric acid is added to activate them. Acid activation mainly affects the specific surface area, pore size, and pore volume of the biochar, obtaining a carbon material with a larger BET, which provides more active sites for subsequent lithium ion charging and discharging.
[0018] Preferably, in the step S1, the mass ratio of the phosphoric acid to the biomass carbon is 4 to 10:1.
[0019] By adopting the technical solution, in order to save costs, dilute phosphoric acid with a concentration of 20% is used, and the mass ratio of dilute phosphoric acid to biochar is 20-50:1; if concentrated phosphoric acid with a concentration of 85% is used, the mass ratio of concentrated phosphoric acid to biochar is 5-20:1.
[0020] Preferably, the step S2 comprises the following steps:
[0021] 1): Add 0.5g to 1.5g of carbon nanotubes into 50ml of strong acid solution;
[0022] 2): After the strong acid solution is stirred in a water bath, it is filtered and washed with deionized water until it becomes neutral, and the washed product is dried to obtain oxidized carbon nanotubes CNTs-COOH;
[0023] 3): Add 12ml-18ml SOCl2 to 0.5g-1.5g CNTs-COOH, stir in a water bath, filter and wash with deionized water until neutral, dry the washed product to obtain CNTs-COCl product;
[0024] 4): 8 g to 12 g of pentaborane is added dropwise to the CNTs-COCl product, stirred in a water bath, filtered, washed with deionized water until neutral, and dried to obtain boron-doped carbon nanotubes B-CNTs.
[0025] By adopting the technical solution, boron-grafted carbon nanotubes are prepared as dopants, which further improve the electrochemical performance of lithium iron phosphate, especially the high-rate performance.
[0026] Preferably, in order to further improve the doping effect, in the step 1), the strong acid solution is prepared by mixing concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1.
[0027] Preferably, in step S3, based on the total mass of the suspension as 100wt%, the mass ratio of the activated biomass carbon, boron-doped carbon nanotubes and sulfur source is 8wt% to 12wt%: 1wt% to 5wt%: 1wt% to 1.3wt%, and the remainder is iron source, phosphorus source and lithium source.
[0028] Preferably, in step S3, the iron source and phosphorus source are iron phosphate; and the lithium source is lithium carbonate.
[0029] Preferably, in step S3, the sulfur source is at least one of ammonium thiosulfate and ammonium sulfide.
[0030] Preferably, in step S3, the lithium-iron molar ratio of the added iron phosphate and lithium carbonate is 1.05-1.1:1.
[0031] Preferably, in step S3, the solid content of the suspension slurry is 30% to 40%.
[0032] Preferably, in step S4, the spray drying temperature is 170°C to 200°C; the high temperature sintering temperature is 720°C to 800°C, and the sintering time is 4h to 12h.
[0033] The technical solution of the embodiment of the present invention has at least the following advantages and beneficial effects:
[0034] 1. The present invention uses cheap biochar as raw material, which reduces the raw material cost and production cost; at the same time, the biochar itself has nitrogen source and carbon source, which saves the cost of adding nitrogen source separately. The nitrogen source and carbon source will form a continuous conductive electron layer after high-temperature sintering, providing a channel for lithium ion deintercalation and improving its electrical properties;
[0035] 2. The present invention grafts boron onto carbon nanotubes, which can make boron doping in lithium iron phosphate more uniform; in addition, the addition of carbon nanotubes can increase the conductivity of lithium iron phosphate and further increase the electrochemical properties of lithium iron phosphate, especially the high rate performance;
[0036] 3. The carbon nanotubes of the present invention can improve the cycle stability at high rates. The carbon nanotubes have high electrical conductivity and can form a three-dimensional conductive network structure between lithium iron phosphate particles, which facilitates the transmission of electrons and lithium ions, reduces the impedance of lithium iron phosphate, and improves the rate performance of lithium iron phosphate.
[0037] 4. The addition of nitrogen, sulfur and boron in the present invention can make the carbon coating on the surface of lithium iron phosphate more uniform, further improving the electrical properties of lithium iron phosphate. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0039] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.
[0040] Example 1
[0041] A method for preparing sulfur, nitrogen and boron co-doped lithium iron phosphate comprises the following steps:
[0042] S1: activating the biochar; adding phosphoric acid to the biochar for activation, wherein the phosphoric acid is diluted phosphoric acid with a concentration of 20%, and the mass ratio of the diluted phosphoric acid to the biochar is 35:1;
[0043] S2: Preparation of boron-doped carbon nanotubes;
[0044] 1): Add 1g of carbon nanotubes into 50ml of a strong acid solution, wherein the strong acid solution is prepared by mixing concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1;
[0045] 2): Stir the strong acid solution for 2 hours in a water bath at 80°C to 90°C, filter and wash with deionized water until neutral, and dry the washed product in an oven at 80°C for 20 hours to obtain oxidized carbon nanotubes CNTs-COOH;
[0046] 3): Add 15 ml SOCl2 to 1 g CNTs-COOH, stir the mixture in a water bath at 50°C to 70°C for 2 h, filter the solution and wash with deionized water until neutral, dry the washed product in a vacuum drying oven at 60°C for 20 h to obtain CNTs-COCl product;
[0047] 4): 10 g of pentaborane was added dropwise to the CNTs-COCl product, the mixed solution was stirred for 4 h in a water bath at 70° C. to 90° C., the solution was filtered and washed with deionized water until neutral, and the product was placed in a vacuum drying oven and dried at 100° C. for 12 h to obtain boron-doped carbon nanotubes B-CNTs;
[0048] S3: The activated biomass carbon, boron-doped carbon nanotubes, iron source, phosphorus source, lithium source and sulfur source are mixed to obtain a suspension, wherein the total mass of the suspension is 100wt%, the mass ratio of the activated biomass carbon, boron-doped carbon nanotubes and sulfur source is 10wt%:3wt%:1.15wt%, and the remainder is iron phosphate and lithium carbonate; the lithium-iron molar ratio of the added iron phosphate and lithium carbonate is 1.075:1; the sulfur source is a mixture of ammonium thiosulfate and ammonium sulfide;
[0049] S4: ball milling, spray drying and high-temperature sintering the suspension to obtain sulfur, nitrogen and boron co-doped lithium iron phosphate; the spray drying temperature is 185° C.; the high-temperature sintering temperature is 760° C., and the sintering time is 8 hours;
[0050] S5: Preparation of lithium iron phosphate cathode material
[0051] The prepared sulfur, nitrogen and boron co-doped lithium iron phosphate, conductive agent carbon black, binder polyvinylidene fluoride (PVDF), and solvent N-methylpyrrolidone were uniformly mixed to prepare electrode slurry, which was then coated, cut, and vacuum dried before being assembled into button batteries for electrochemical performance testing.
[0052] The test adopts constant current charge and discharge, and its parameters are set as current density of 50mAg, 10 cycles; current density of 100mA / g, 10 cycles; current density of 200mAg, 10 cycles; current density of 500mAg, 10 cycles; current density of 1000mA / g, 10 cycles; current density of 50mAg, 10 cycles. The test voltage is 2.0~3.75V, and the scan rate is 0.1mV / s.
[0053] In this embodiment, the first discharge capacity at a rate of 0.1C is 163 mAh / g, and the charge and discharge efficiency is 98.5%. At a rate of 8C, the discharge capacity is 150 mAh / g, and the capacity retention rate after 200 cycles is 98.8%.
[0054] Example 2
[0055] The only difference between this embodiment and embodiment 1 is that, in this embodiment, based on the total mass of the suspension as 100wt%, the mass ratio of the activated biomass carbon, boron-doped carbon nanotubes and sulfur source is 12wt%:5wt%:1.3wt%, and the remainder is iron phosphate and lithium carbonate; the lithium-iron molar ratio of the added iron phosphate and lithium carbonate is 1.075:1.
[0056] In this embodiment, the first discharge capacity at a rate of 0.1C is 164 mAh / g, and the charge and discharge efficiency is 98.4%. At a rate of 8C, the discharge capacity is 152 mAh / g, and the capacity retention rate after 200 cycles is 98.2%.
[0057] Example 3
[0058] The only difference between this embodiment and embodiment 1 is that, in this embodiment, based on the total mass of the suspension as 100wt%, the mass ratio of the activated biomass carbon, boron-doped carbon nanotubes and sulfur source is 8wt%:1wt%:1wt%, and the remainder is iron phosphate and lithium carbonate; the lithium-iron molar ratio of the added iron phosphate and lithium carbonate is 1.075:1.
[0059] In this embodiment, the first discharge capacity at a rate of 0.1C is 160 mAh / g, and the charge and discharge efficiency is 98.3%. At a rate of 8C, the discharge capacity is 148 mAh / g, and the capacity retention rate after 200 cycles is 98.5%.
[0060] Example 4
[0061] The only difference between this embodiment and embodiment 1 is that, in this embodiment, based on the total mass of the suspension as 100wt%, the mass ratio of the activated biomass carbon, boron-doped carbon nanotubes and sulfur source is 12wt%: 1wt%: 1.3wt%, and the remainder is iron phosphate and lithium carbonate; the lithium-iron molar ratio of the added iron phosphate and lithium carbonate is 1.075:1.
[0062] In this embodiment, the first discharge capacity at a rate of 0.1C is 164 mAh / g, and the charge and discharge efficiency is 98.4%. At a rate of 8C, the discharge capacity is 147 mAh / g, and the capacity retention rate after 200 cycles is 95.2%.
[0063] Example 5
[0064] The only difference between this embodiment and embodiment 1 is that, in this embodiment, based on the total mass of the suspension as 100wt%, the mass ratio of the activated biomass carbon, boron-doped carbon nanotubes and sulfur source is 8wt%:5wt%:1wt%, and the remainder is iron phosphate and lithium carbonate; the lithium-iron molar ratio of the added iron phosphate and lithium carbonate is 1.075:1.
[0065] In this embodiment, the first discharge capacity at a rate of 0.1C is 161 mAh / g, and the charge and discharge efficiency is 97.8%. At a rate of 8C, the discharge capacity is 151 mAh / g, and the capacity retention rate after 200 cycles is 98.5%.
[0066] Example 6
[0067] The only difference between this embodiment and embodiment 1 is that, in this embodiment, based on the total mass of the suspension as 100wt%, the mass ratio of the activated biomass carbon, boron-doped carbon nanotubes and sulfur source is 10wt%:3wt%:1.15wt%, and the remainder is iron phosphate and lithium carbonate; the lithium-iron molar ratio of the added iron phosphate and lithium carbonate is 1.05:1.
[0068] In this embodiment, the first discharge capacity at a rate of 0.1C is 162 mAh / g, and the charge and discharge efficiency is 98.1%. At a rate of 8C, the discharge capacity is 151 mAh / g, and the capacity retention rate after 200 cycles is 98.3%.
[0069] Example 7
[0070] The only difference between this embodiment and embodiment 1 is that, in this embodiment, based on the total mass of the suspension as 100wt%, the mass ratio of the activated biomass carbon, boron-doped carbon nanotubes and sulfur source is 10wt%:3wt%:1.15wt%, and the remainder is iron phosphate and lithium carbonate; the lithium-iron molar ratio of the added iron phosphate and lithium carbonate is 1.1:1.
[0071] In this embodiment, the first discharge capacity at a rate of 0.1C is 161 mAh / g, and the charge and discharge efficiency is 98.6%. At a rate of 8C, the discharge capacity is 151 mAh / g, and the capacity retention rate after 200 cycles is 98.7%.
[0072] Comparative Example 1
[0073] The difference between this comparative example and Example 1 is that in this comparative example, the biochar is directly added without being activated by phosphoric acid, and is then activated during the subsequent high-temperature sintering.
[0074] In this comparative example, the first discharge capacity at a rate of 0.1C is 148 mAh / g, and the charge and discharge efficiency is 98%. At a rate of 8C, the discharge capacity is 139 mAh / g, and the capacity retention rate after 200 cycles is 97.5%.
[0075] Comparative Example 2
[0076] The only difference between this comparative example and Example 1 is that in this comparative example, the pentaborane is not grafted via carbon nanotubes, but is directly added simultaneously with the biochar activated with phosphoric acid.
[0077] In this comparative example, the first discharge capacity at 0.1C rate is 158 mAh / g, the charge and discharge efficiency is 97.5%, at 8C rate, the discharge capacity is 147 mAh / g, and the capacity retention rate after 200 cycles is 98.2%.
[0078] The relevant data of Examples 1-7 are shown in Table 1 as follows:
[0079] Table 1. Doping related addition amounts and electrochemical performance of Examples 1-7
[0080]
[0081] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing sulfur, nitrogen and boron co-doped lithium iron phosphate, characterized in that: The steps include: S1: Activate the biochar; S2: Preparation of boron-doped carbon nanotubes; S3: mixing the activated biomass carbon, boron-doped carbon nanotubes, iron source, phosphorus source, lithium source and sulfur source to obtain a suspension; S4: ball-milling, spray-drying and sintering the suspension to obtain sulfur-, nitrogen- and boron-coated lithium iron phosphate.
2. The method for preparing sulfur, nitrogen and boron co-doped lithium iron phosphate according to claim 1, characterized in that: In the step S1, phosphoric acid is added to the biochar for activation treatment.
3. The method for preparing sulfur, nitrogen and boron co-doped lithium iron phosphate according to claim 2, characterized in that: In the step S1, the mass ratio of the phosphoric acid to the biomass carbon is 4 to 10:
1.
4. A method for preparing sulfur, nitrogen and boron co-doped lithium iron phosphate according to any one of claims 1 to 3, characterized in that: The step S2 comprises the following steps: 1): Add 0.5g to 1.5g of carbon nanotubes into 50ml of strong acid solution; 2): After stirring the strong acid solution in a water bath, the solution is filtered and washed with deionized water until it becomes neutral, and the washed product is dried to obtain oxidized carbon nanotubes; 3): Add 12 ml to 18 ml of SOCl2 to 0.5 g to 1.5 g of oxidized carbon nanotubes, stir in a water bath, filter and wash with deionized water until neutral, and dry the washed product to obtain CNTs-COCl product; 4) 8 g to 12 g of pentaborane is added dropwise to the CNTs-COCl product, stirred in a water bath, filtered, washed with deionized water until neutral, and dried to obtain boron-doped carbon nanotubes.
5. The method for preparing sulfur, nitrogen and boron co-doped lithium iron phosphate according to claim 4, characterized in that: In the step 1), the strong acid solution is prepared by mixing concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:
1.
6. A method for preparing sulfur, nitrogen and boron co-doped lithium iron phosphate according to any one of claims 1 to 3 and 5, characterized in that: In step S3, based on the total mass of the suspension as 100wt%, the mass ratio of the activated biomass carbon, boron-doped carbon nanotubes and sulfur source is 8wt%-12wt%: 1wt%-5wt%: 1wt%-1.3wt%, and the remainder is iron source, phosphorus source and lithium source.
7. A method for preparing sulfur, nitrogen and boron co-doped lithium iron phosphate according to any one of claims 1 to 3 and 5, characterized in that: In step S3, the iron source and phosphorus source are iron phosphate; and the lithium source is lithium carbonate.
8. The method for preparing sulfur, nitrogen and boron co-doped lithium iron phosphate according to claim 7, characterized in that: In the step S3, the lithium iron molar ratio of the added iron phosphate and lithium carbonate is 1.05-1.1:
1.
9. A method for preparing sulfur, nitrogen and boron co-doped lithium iron phosphate according to any one of claims 1 to 3, 5 and 8, characterized in that: In the step S3, the solid content of the suspension slurry is 30% to 40%.
10. A method for preparing sulfur, nitrogen and boron co-doped lithium iron phosphate according to any one of claims 1 to 3, 5 and 8, characterized in that: In the step S4, the spray drying temperature is 170°C to 200°C; the high temperature sintering temperature is 720°C to 800°C, and the sintering time is 4h to 12h.
Citation Information
Patent Citations
Nitrogen-phosphorus-sulfur co-doping composite carbon material, preparation method of composite carbon material and lithium ion battery
CN108493424A
Nitrogen-doped carbon modified lithium iron phosphate positive electrode material
CN115133010A
Composite positive electrode material and battery comprising same
CN115241431A
Nitrogen-sulfur-boron three-doped carbon quantum dot coated lithium manganese iron phosphate positive electrode material and preparation method and application thereof
CN118156448A
Cited By
High-conductivity lithium iron phosphate material and preparation method thereof
CN119581532A