Preparation method of layered carbon-derived wave-absorbing material

The preparation of layered carbon-derived absorbing materials through the ice template method solves the problem of easy agglomeration of materials and impedance mismatch, achieves good dispersion and impedance matching, significantly improves the electromagnetic wave absorption performance, and is suitable for lightweight and efficient electromagnetic wave absorption application.

CN118894520APending Publication Date: 2024-11-05ZHONGBEI UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411056794.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing layered carbon-derived absorbing materials are prone to agglomeration, disorderly arrangement and mismatched impedances, which affect their electromagnetic wave absorption performance.

Method used

ZIF-8 nanoparticles were rearranged and carbonized by ice template method to prepare layered metal organic frame carbon-derived micron-sized materials, and the rapid freezing process was used to form good dispersion and pore structure to improve impedance matching.

Benefits of technology

The prepared layered carbon-derived absorbing material has good dispersion and impedance matching characteristics, which significantly improves the electromagnetic wave absorption performance. The frequency band width with a reflection loss intensity of less than -10 dB is expanded, and is suitable for lightweight and efficient electromagnetic wave absorption applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894520A_ABST
    Figure CN118894520A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a layered carbon-derived wave-absorbing material, belongs to the technical field of electromagnetic absorbing materials, and can solve the problems that the layered carbon-derived wave-absorbing material prepared by the existing method is easy to agglomerate, disordered in arrangement and mismatched in impedance. The layered metal organic framework carbon-derived micron-sized material is obtained. The layered carbon derivative material obtained by the method has good chemical homogeneity, and the impedance matching is effectively improved due to the large specific surface area and the high porosity of the layered carbon derivative material, so that the microwave absorption performance is remarkably improved. The material prepared by the method is used for preparing a light and efficient electromagnetic wave absorbing coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electromagnetic absorption materials, and in particular relates to a method for preparing a layered carbon-derived absorbing material. Background Art

[0002] The development of electronic equipment and radio communications has brought great convenience to human production and life. At the same time, the increasingly dense electromagnetic pollution it generates also poses a potential security threat to the normal operation of equipment and human health. In addition, in order to improve the battlefield survivability of high-value military targets and improve the combat effectiveness and combat life of weapons and equipment, there is an urgent need for a lightweight and efficient electromagnetic wave absorber for electromagnetic protection. In summary, the development of new, lightweight and efficient electromagnetic protection materials plays an important role in all areas of the national economy and national defense construction. At present, common electromagnetic protection materials include electromagnetic shielding materials and electromagnetic wave absorbing materials. Usually, electromagnetic shielding materials have poor impedance matching characteristics, and electromagnetic waves are difficult to enter the interior of electromagnetic shielding materials and are lost, which will cause electromagnetic pollution to re-enter the outside world and cause secondary pollution. Electromagnetic wave absorbing materials can allow most electromagnetic waves to enter the interior of the material and can convert electromagnetic energy into other forms of energy such as heat energy, which fundamentally alleviates electromagnetic pollution and has been widely studied in recent years. At present, various electromagnetic wave absorbing materials, such as magnetic metals / ferrites, metal oxides / sulfides, conductive polymers, carbon materials, etc., have been widely used in the prevention and elimination of electromagnetic pollution. Metal-organic framework derivatives have very strong dielectric loss capacity due to their good conductivity, large specific surface area, complex interface and adjustable structure. At the same time, they have low density and high chemical stability, and have potential applications in the field of electromagnetic wave absorption. Studies have found that in metal-organic framework derivative composites, the structure of the material has a very important influence on the electromagnetic absorption performance of the composite. Recently, researchers have prepared absorbing materials such as core-shell structure, porous structure and chiral helical structure by different methods, and these composites have strong attenuation characteristics for incident electromagnetic waves. However, these composites show serious agglomeration phenomenon, which is not conducive to performance reproducibility. Summary of the invention

[0003] The invention aims at solving the problems of easy agglomeration, disordered arrangement and impedance mismatch of layered carbon-derived absorbing materials prepared by existing methods, and provides a method for preparing the layered carbon-derived absorbing materials.

[0004] The present invention rearranges ZIF-8 nanoparticles by an ice template method and obtains a layered metal organic framework carbon-derived micron-sized material by carbonization, which specifically includes the following steps: The first step is to prepare ZIF-8 powder: The aqueous solution A of 2-methylimidazole was added to the zinc acetate dihydrate dispersion liquid containing hexadecyltrimethylammonium bromide, and stirred at room temperature for 3 hours at a stirring speed of 400 r / min to obtain a uniform solution, which was washed with water after centrifugation and dried at 60°C for 12 hours to obtain a white dodecahedral ZIF-8 powder; Alternatively, zinc nitrate hexahydrate is dispersed in deionized water containing hexadecyltrimethylammonium bromide, and then an aqueous solution B of 2-methylimidazole is added, and the mixture is stirred vigorously at room temperature for 5 minutes at a stirring speed of 1000 r / min, and allowed to stand for 3 hours. After centrifugation, the mixture is washed with alcohol and dried at 60°C for 12 hours to obtain a white cubic ZIF-8 powder; In the second step, the ZIF-8 powder obtained in the first step is added to ultrapure water to form a mixed solution, which is ultrasonically treated to form a colloid, and then quickly frozen into a solid, and then placed in a freeze dryer for freeze drying to obtain an intermediate product; In the third step, the intermediate product obtained in the second step is calcined at a high temperature under a nitrogen atmosphere to obtain a layered carbon-derived absorbing material.

[0005] Furthermore, in the first step, the volume ratio of the aqueous solution A of 2-methylimidazole to the zinc acetate dihydrate dispersion liquid containing hexadecyltrimethylammonium bromide is 20-30:20-30.

[0006] Furthermore, in the aqueous solution A of 2-methylimidazole in the first step, the mass of 2-methylimidazole is 5-6 g; in the zinc acetate dihydrate dispersion liquid containing hexadecyltrimethylammonium bromide, the mass of hexadecyltrimethylammonium bromide is 3-7 mg, and the mass of zinc acetate dihydrate is 1-2 g.

[0007] Furthermore, in the first step, the mass of the zinc nitrate hexahydrate is 0.07-0.13 g; in the deionized water containing hexadecyltrimethylammonium bromide, the amount of deionized water is 18-24 mL, and the amount of hexadecyltrimethylammonium bromide is 6-12 mg.

[0008] Furthermore, in the aqueous solution B of 2-methylimidazole in the first step, the amount of the aqueous solution of 2-methylimidazole is 15-21 mL, wherein the mass of 2-methylimidazole is 1.5-2.1 g.

[0009] Furthermore, in the mixed solution in the second step, the mass of ZIF-8 powder is 295-305 mg, and the volume of ultrapure water is 15 mL or 30 mL.

[0010] Furthermore, in the second step, the ultrasonic frequency is 40KHz, and the ultrasonic time is 2-3h.

[0011] Furthermore, the freeze drying in the second step uses a cold trap of a cold dryer, the temperature of the cold trap of the cold dryer is -50~-70°C, the vacuum degree is 5~30Pa, and the freeze drying time is 12~24h.

[0012] Furthermore, the heating rate of the high temperature calcination in the third step is 2°C / min, the calcination temperature is 800°C, and the calcination time is 3h.

[0013] In the layered carbon-derived absorbing material formed by the method provided by the present invention, due to the directional growth of the ice template during the rapid freezing process, the ZIF-8 colloid in the aqueous solution is directional and arranged, and after freeze drying, a layered ZIF-8 powder is formed, which ensures good dispersibility of the composite material. In addition, the mutual contact of the stacked ZIF-8 particles inhibits the collapse of the structure during the carbonization process, forming a large number of pores, and the introduction of these pores significantly improves the impedance matching of the material.

[0014] The layered carbon derivative material prepared by the present invention can be used in an electromagnetic wave absorber. The absorber includes the layered carbon derivative electromagnetic wave absorber and paraffin. The mass percentage of the layered carbon derivative material in the absorber can be adjusted according to actual needs.

[0015] Preferably, the mass fraction of the cubic layered carbon-derived electromagnetic wave absorbing material in the absorber is 50%. At this filler ratio, the frequency range in which the reflection loss intensity is less than -10 dB is 4.56-18.0 GHz.

[0016] The beneficial effects of the present invention are: 1. In the prepared layered carbon-derived absorbing material, the ZIF-8 particles are stacked in a directional manner, presenting a single-layer or double-layer stacking morphology and then carbonized, ensuring good dispersion of the composite material.

[0017] 2. In the prepared layered carbon-derived absorbing material, the particles are stacked on each other, avoiding the collapse of the structure during the carbonization process, forming a large number of pores, and significantly improving the impedance matching of the composite material.

[0018] 3. It has excellent wave absorption performance and can effectively absorb the reflection loss intensity less than the bandwidth of -10 dB. The prepared absorber is thin, light and has high absorption intensity. It has broad application prospects in the fields of electromagnetic wave absorption in the communication technology field, prevention of electromagnetic leakage, and electromagnetic protection of high-precision instruments.

[0019] The layered carbon-derived absorbing material prepared by the present invention presents a layered stacked morphology, is uniform in size, has good dispersibility, and has excellent impedance matching characteristics. The maximum reflection loss of the cubic layered stacked carbon derivative can reach -82.7245 dB. When the thickness of the absorber is 2.38 mm, the bandwidth in which the reflection loss is less than -10 dB can reach about 6.20 GHz, ranging from 11.80 to 18.00 GHz.

[0020] In summary, the present invention prepares a layered carbon-derived electromagnetic wave absorbing material having good impedance matching characteristics. The ZIF-8 particles are rearranged and carbonized by the ice template method, so that the composite material presents a layered stacking morphology, ensuring its good dispersibility. In the obtained layered carbon-derived nanotube composite material, the carbon-derived crystal structure is amorphous, which significantly improves the impedance matching characteristics of the composite material, so that the composite material has broad application prospects in electromagnetic absorption.

[0021] The material prepared by the invention is used for making a light and efficient wave absorbing coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a scanning electron microscope image of the layered cubic derivative absorbing material prepared in Example 1; Figure 2 This is a transmission electron microscope image of the layered cubic derivative absorbing material prepared in Example 1; Figure 3 The XRD patterns of the layered cubic derivative absorbing material and the comparative sample prepared in Example 1, wherein curve a is the XRD pattern of the comparative sample; curve b is the XRD pattern of the layered cubic derivative absorbing material; Figure 4 The Raman spectra of the layered cubic derivative absorbing material and the comparative sample prepared in Example 1, wherein curve a is the Raman spectrum of the comparative sample; curve b is the Raman spectrum of the layered cubic derivative electromagnetic wave absorbing material; Figure 5 Graphs showing the real part of the dielectric constants of the layered cubic derivative absorbing material and the comparative sample prepared in Example 1, wherein curve a is the real part of the dielectric constant of the comparative sample; curve b is the real part of the dielectric constant of the layered cubic derivative absorbing material; Figure 6 Graphs showing the imaginary part of the dielectric constant of the layered cubic derivative absorbing material and the comparative sample prepared in Example 1, wherein curve a is the imaginary part of the dielectric constant of the comparative sample; curve b is the imaginary part of the dielectric constant of the layered cubic derivative absorbing material; Figure 7The Δ function graphs of the layered cubic derivative absorbing material and the comparative sample prepared in Example 1, wherein Figure (a) is the Δ function graph of the comparative sample; Figure (b) is the Δ function graph of the layered cubic derivative absorbing material; Figure 8 The wave impedance curves of the layered cubic derivative absorbing material and the comparative sample prepared in Example 1, a is the wave impedance curve of the comparative sample; b is the wave impedance curve of the layered cubic derivative electromagnetic wave absorbing material; Fig. 9 This is a three-dimensional graph of the reflection loss of the layered cubic derivative absorbing material prepared in Example 1. DETAILED DESCRIPTION

[0023] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any combination of the specific implementation modes.

[0024] Example 1 A method for preparing a layered cubic derivative absorbing material comprises the following steps: S1. Add the aqueous solution A of 2-methylimidazole to the zinc acetate dihydrate dispersion liquid containing hexadecyltrimethylammonium bromide, stir at room temperature for 3 hours at a stirring speed of 400 r / min to obtain a uniform solution, wash with deionized water after centrifugation, and dry at 60°C for 12 hours to obtain a white dodecahedral ZIF-8 powder; The amount of dimethylimidazole aqueous solution A is 25 ml, of which the mass of dimethylimidazole is 5.6 g; The amount of zinc acetate dihydrate dispersion containing hexadecyltrimethylammonium bromide is 25 ml, wherein the amount of zinc acetate dihydrate is 1.5 g and the amount of hexadecyltrimethylammonium bromide is 5 mg; Alternatively, zinc nitrate hexahydrate is dispersed in deionized water containing hexadecyltrimethylammonium bromide, and then an aqueous solution B of 2-methylimidazole is added, and the mixture is stirred vigorously at room temperature for 5 minutes at a stirring speed of 1000 r / min, and allowed to stand for 3 hours. After centrifugation, the mixture is washed with ethanol, and dried at 60°C for 12 hours to obtain a white cubic ZIF-8 powder; The amount of deionized water used was 21 mL, the amount of zinc nitrate hexahydrate used was 0.1 g, and the amount of hexadecyltrimethylammonium bromide used was 9 mg; The amount of 2-methylimidazole aqueous solution B used is 18 mL, of which the mass of 2-methylimidazole is 1.8 g; S2, adding the white powder obtained in S1 to ultrapure water to form a mixed solution, ultrasonically treating until a colloid is formed, then placing it in liquid nitrogen or a cold trap of a freeze dryer to quickly freeze it into a solid, and then placing it in a freeze dryer for freeze drying to obtain an intermediate product; The concentration of the mixed solution is 20 mg / ml, including 15 ml of deionized water and 300 mg of sample; The ultrasonic frequency was controlled to 40 KHz and the ultrasonic time was 2-3 h; The cold trap temperature of the freeze dryer is -68.4℃, the vacuum degree of the freeze dryer is 6pa, and the freeze drying time is 18 hours; S3, calcining the intermediate product obtained in S2 at high temperature under a nitrogen atmosphere, controlling the heating rate to be 2 °C / min, the calcination temperature to be 800 °C, and the calcination time to be 3 h, to obtain a layered cubic carbon-derived absorbing material; The comparative sample is a white powder of S1, which is calcined at high temperature to obtain a layered dodecahedron derivative. The calcination process is consistent with the above, that is, the heating rate is 2 °C / min, the calcination temperature is 800 °C, and the calcination time is 3 h.

[0025] Figure 1 This is a scanning electron microscope image of the layered cubic derivative absorbing material prepared in Example 1; it can be seen from the figure that the obtained carbon microcage encapsulated carbon nanotube composite material is stacked by cubes to form a large layered stacked material with a particle size distribution of 110 nm and good dispersibility.

[0026] Figure 2 This is a transmission electron microscope image of the layered cubic derivative absorbing material prepared in Example 1; it can be seen from the image that the obtained cubes are stacked into a double-layer structure; Figure 3 The XRD graphs of the layered cubic derivative absorbing material and the comparative sample prepared in Example 1, wherein curve a is the XRD of the comparative sample; curve b is the XRD of the layered cubic derivative absorbing material. By comparing the X-ray diffraction standard card, it can be seen that although the layered cubic derivative absorbing material and the comparative sample both contain the diffraction peak of amorphous carbon, the diffraction peak of the comparative sample is stronger than that of the layered cubic derivative electromagnetic wave absorbing material, indicating that the graphitization degree of the layered cubic derivative electromagnetic wave absorbing material is lower than that of the comparative sample.

[0027] Figure 4 The Raman spectra of the layered cubic derivative absorbing material and the comparative sample prepared in Example 1, curve a in the figure is the Raman spectrum of the comparative sample; curve b is the Raman spectrum of the layered cubic derivative electromagnetic wave absorbing material. I D / I G The value is higher than that of the comparison sample I D / I GThe large value further indicates that the graphitization degree of the layered cubic derivative absorber is lower than that of the comparison sample.

[0028] Figure 5 The graph is a real part curve of the dielectric constant of the layered cubic derivative absorbing material and the comparative sample prepared in Example 1, wherein curve a is the real part curve of the dielectric constant of the comparative sample; and curve b is the real part curve of the dielectric constant of the layered cubic derivative absorbing material. It can be seen from the graph that the real part value of the dielectric constant of the layered cubic derivative absorbing material is lower than that of the comparative sample, because the graphitization degree of the layered cubic derivative absorbing material is lower than that of the comparative sample.

[0029] Figure 6 The imaginary part curves of dielectric constants of the layered cubic derivative absorbing material and the comparative sample prepared in Example 1 are shown in FIG. Curve a is the imaginary part curve of dielectric constants of the comparative sample; Curve b is the imaginary part curve of dielectric constants of the layered cubic derivative absorbing material. It can be seen from the figure that the imaginary part value of dielectric constants of the layered cubic derivative absorbing material is lower than that of the comparative sample, because the use of the layered cubic derivative reduces the conductivity of the composite material.

[0030] Figure 7 The Δ function graphs of the layered cubic derivative absorbing material and the comparative sample prepared in Example 1 are shown in Figure (a) for the comparative sample and Figure (b) for the layered cubic derivative absorbing material. It can be seen from the figure that the area below 0.4 in the Δ function graph of the layered cubic derivative absorbing material is much larger than the area below 0.4 in the Δ function graph of the comparative sample, indicating that the layered cubic derivative absorbing material can significantly improve impedance matching.

[0031] Figure 8 The wave impedance curves of the layered cubic derivative absorbing material and the comparative sample prepared in Example 1, a is the wave impedance curve of the comparative sample; b is the wave impedance curve of the layered cubic derivative electromagnetic wave absorbing material. It can be seen from the figure that the wave impedance value of the layered cubic derivative absorbing material is higher than that of the comparative sample, further indicating that the use of the layered cubic derivative can significantly improve impedance matching.

[0032] Fig. 9The three-dimensional graph of reflection loss of the layered cubic derivative absorbing material prepared in Example 1, wherein the frequency is 2.0-18.0 GHz and the thickness is 1.0-5.0 mm. It can be seen from the figure that the composite material has a maximum reflection loss value of -82.7245 dB at a frequency of 9.5 GHz; and when the thickness is in the range of 1.0-5.0 mm, the frequency band in which its reflection loss is less than -10 dB is 4.56-18.0 GHz (about 13.44 GHz), which can achieve most of the C-band, X-band and Ku-band coverage, indicating that the layered cubic derivative absorbing material has excellent electromagnetic wave absorption capability.

[0033] Example 2 A method for preparing a layered cubic derivative absorbing material comprises the following steps: S1. Add the aqueous solution A of 2-methylimidazole to the zinc acetate dihydrate dispersion liquid containing hexadecyltrimethylammonium bromide, stir at room temperature for 3 hours at a stirring speed of 400 r / min to obtain a uniform solution, wash with deionized water after centrifugation, and dry at 60°C for 12 hours to obtain a white dodecahedral ZIF-8 powder; The amount of dimethylimidazole aqueous solution A is 20 ml, of which the mass of dimethylimidazole is 5 g; The amount of zinc acetate dihydrate dispersion containing hexadecyltrimethylammonium bromide is 20 ml, wherein the amount of zinc acetate dihydrate is 1 g and the amount of hexadecyltrimethylammonium bromide is 3 mg; Alternatively, zinc nitrate hexahydrate is dispersed in deionized water containing hexadecyltrimethylammonium bromide, and then an aqueous solution B of 2-methylimidazole is added, and the mixture is stirred vigorously at room temperature for 5 minutes at a stirring speed of 1000 r / min, and allowed to stand for 3 hours. After centrifugation, the mixture is washed with ethanol, and dried at 60°C for 12 hours to obtain a white cubic ZIF-8 powder; The amount of deionized water used was 18 mL, the amount of zinc nitrate hexahydrate used was 0.07 g, and the amount of hexadecyltrimethylammonium bromide used was 6 mg; The amount of 2-methylimidazole aqueous solution B used is 15 mL, of which the mass of 2-methylimidazole is 1.5 g; S2, adding the white powder obtained in S1 to ultrapure water to form a mixed solution, ultrasonically treating until a colloid is formed, then placing it in liquid nitrogen or a cold trap of a freeze dryer to quickly freeze it into a solid, and then placing it in a freeze dryer for freeze drying to obtain an intermediate product; The concentration of the mixed solution is 19.67 mg / ml, including 15 ml of deionized water and 295 mg of sample; The ultrasonic frequency was controlled to 40 KHz and the ultrasonic time was 2-3 h; The cold trap temperature of the freeze dryer is -50°C, the vacuum degree of the freeze dryer is 5 Pa, and the freeze drying time is 12 hours; S3. The intermediate product obtained in S2 is calcined at high temperature under a nitrogen atmosphere, with the heating rate controlled at 2 °C / min, the calcination temperature at 800 °C, and the calcination time at 3 h to obtain a layered cubic carbon-derived absorbing material.

[0034] Example 3 A method for preparing a layered cubic derivative absorbing material comprises the following steps: S1. Add the aqueous solution A of 2-methylimidazole to the zinc acetate dihydrate dispersion liquid containing hexadecyltrimethylammonium bromide, stir at room temperature for 3 hours at a stirring speed of 400 r / min to obtain a uniform solution, wash with deionized water after centrifugation, and dry at 60°C for 12 hours to obtain a white dodecahedral ZIF-8 powder; The amount of dimethylimidazole aqueous solution A is 30 ml, of which the mass of dimethylimidazole is 6 g; The amount of zinc acetate dihydrate dispersion containing hexadecyltrimethylammonium bromide is 30 ml, wherein the amount of zinc acetate dihydrate is 2 g and the amount of hexadecyltrimethylammonium bromide is 7 mg; Alternatively, zinc nitrate hexahydrate is dispersed in deionized water containing hexadecyltrimethylammonium bromide, and then an aqueous solution B of 2-methylimidazole is added, and the mixture is stirred vigorously at room temperature for 5 minutes at a stirring speed of 1000 r / min, and allowed to stand for 3 hours. After centrifugation, the mixture is washed with ethanol, and dried at 60°C for 12 hours to obtain a white cubic ZIF-8 powder; The amount of deionized water used was 24 mL, the amount of zinc nitrate hexahydrate used was 0.13 g, and the amount of hexadecyltrimethylammonium bromide used was 12 mg; The amount of 2-methylimidazole aqueous solution B used is 21 mL, of which the mass of 2-methylimidazole is 2.1 g; S2, adding the white powder obtained in S1 to ultrapure water to form a mixed solution, ultrasonically treating until a colloid is formed, then placing it in liquid nitrogen or a cold trap of a freeze dryer to quickly freeze it into a solid, and then placing it in a freeze dryer for freeze drying to obtain an intermediate product; The concentration of the mixed solution is 20.33 mg / ml, including 15 ml of deionized water and 305 mg of sample; The ultrasonic frequency was controlled to 40 KHz and the ultrasonic time was 2-3 h; The cold trap temperature of the freeze dryer is -70°C, the vacuum degree of the freeze dryer is 10pa, and the freeze drying time is 20 hours; S3. The intermediate product obtained in S2 is calcined at high temperature under a nitrogen atmosphere, with the heating rate controlled at 2 °C / min, the calcination temperature at 800 °C, and the calcination time at 3 h to obtain a layered cubic carbon-derived absorbing material.

Claims

1. A method for preparing a layered carbon-derived absorbing material, characterized in that: The steps include: The first step is to prepare ZIF-8 powder: The aqueous solution A of 2-methylimidazole was added to the zinc acetate dihydrate dispersion liquid containing hexadecyltrimethylammonium bromide, and stirred at room temperature for 3 hours at a stirring speed of 400 r / min to obtain a uniform solution, which was washed with water after centrifugation and dried at 60°C for 12 hours to obtain a white dodecahedral ZIF-8 powder; Alternatively, zinc nitrate hexahydrate is dispersed in deionized water containing hexadecyltrimethylammonium bromide, and then an aqueous solution B of 2-methylimidazole is added, and the mixture is stirred vigorously at room temperature for 5 minutes at a stirring speed of 1000 r / min, and allowed to stand for 3 hours. After centrifugation, the mixture is washed with alcohol and dried at 60°C for 12 hours to obtain a white cubic ZIF-8 powder; In the second step, the ZIF-8 powder obtained in the first step is added to ultrapure water to form a mixed solution, which is ultrasonically treated to form a colloid, and then quickly frozen into a solid, and then placed in a freeze dryer for freeze drying to obtain an intermediate product; In the third step, the intermediate product obtained in the second step is calcined at a high temperature under a nitrogen atmosphere to obtain a layered carbon-derived absorbing material.

2. The method for preparing a layered carbon-derived absorbing material according to claim 1, characterized in that: In the first step, the volume ratio of the aqueous solution A of 2-methylimidazole to the zinc acetate dihydrate dispersion liquid containing hexadecyltrimethylammonium bromide is 20-30:20-30.

3. The method for preparing a layered carbon-derived absorbing material according to claim 1, characterized in that: In the aqueous solution A of 2-methylimidazole in the first step, the mass of 2-methylimidazole is 5-6 g; in the zinc acetate dihydrate dispersion liquid containing hexadecyltrimethylammonium bromide, the mass of hexadecyltrimethylammonium bromide is 3-7 mg, and the mass of zinc acetate dihydrate is 1-2 g.

4. The method for preparing a layered carbon-derived absorbing material according to claim 1, characterized in that: The mass of the zinc nitrate hexahydrate in the first step is 0.07-0.13 g; in the deionized water containing hexadecyltrimethylammonium bromide, the amount of deionized water used is 18-24 mL, and the amount of hexadecyltrimethylammonium bromide used is 6-12 mg.

5. The method for preparing a layered carbon-derived absorbing material according to claim 1, characterized in that: In the aqueous solution B of 2-methylimidazole in the first step, the amount of the aqueous solution of 2-methylimidazole is 15-21 mL, wherein the mass of 2-methylimidazole is 1.5-2.1 g.

6. The method for preparing a layered carbon-derived absorbing material according to claim 1, characterized in that: In the mixed solution in the second step, the mass of ZIF-8 powder is 295-305 mg, and the volume of ultrapure water is 15 mL or 30 mL.

7. The method for preparing a layered carbon-derived absorbing material according to claim 1, characterized in that: In the second step, the ultrasonic frequency is 40 KHz, and the ultrasonic time is 2-3 hours.

8. The method for preparing a layered carbon-derived absorbing material according to claim 1, characterized in that: The freeze drying in the second step uses a cold trap of a cold dryer, the temperature of the cold trap of the cold dryer is -50~-70°C, the vacuum degree is 5~30Pa, and the freeze drying time is 12~24h.

9. The method for preparing a layered carbon-derived absorbing material according to claim 1, characterized in that: The heating rate of the high temperature calcination in the third step is 2°C / min, the calcination temperature is 800°C, and the calcination time is 3h.

Citation Information

Patent Citations

  • Preparation method of ZIF-67 having multi-level pore structure, and honeycomb-like carbon / cobalt wave-absorbing material preparation method

    CN109293939A

  • One-dimensional N-doped carbon nanorod material as well as preparation method and application thereof

    CN114286608A

  • Synthesis method and application of two-dimensional layered hollow carbon nanoparticle array superstructure

    CN115744876A

  • Derivative wave-absorbing material based on Co-ZIF-L and preparation method

    CN116656318A

  • Method for preparing two-dimensional organic metal framework carbon fluoride positive electrode material through ice template method

    CN116854077A