Lithium-based montmorillonite inorganic modified material, preparation method and application of lithium-based montmorillonite inorganic modified material in ionic conduction technology
Lithium montmorillonite was prepared by inserting anhydrous lithium chloride into sodium montmorillonite and modifying by microwave-assisted ultrasound method, which solved the problem of insufficient conductivity of sodium montmorillonite and achieved significant improvement in soil The effect of conductivity.
Patent Information
- Application Number
- CN202410932977.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-05
AI Technical Summary
Many soils have low natural conductivity, which limits their application in improving the conductivity of grounding systems, especially the lack of conductivity of sodium-based montmorillonite, which limits their application in improving the conductivity of soil.
Lithium-based montmorillonite was prepared by intercalating anhydrous lithium chloride in sodium-based montmorillonite and inorganic modification was performed by microwave-assisted ultrasound. After inorganic modification, the mass ratio of montmorillonite and lithium chloride was adjusted. Improves its ionic conductivity.
Significantly improves the ionic conductivity of sodium-based montmorillonite, making its conductivity twice or higher than that of original sodium-based montmorillonite, and exhibits typical temperature and humidity dependence, with increasing conductivity with temperature and humidity Increase and increase.
Smart Images

Figure CN118894534A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ion conduction, and in particular relates to a lithium-based montmorillonite inorganic modified material, a preparation method and application thereof in ion conduction technology. Background Art
[0002] In modern power systems, the performance of grounding devices is critical to the safety and reliability of the system. Good grounding can effectively reduce the risk of electrical accidents caused by lightning, power failures, etc. The correct design of the grounding system depends largely on the soil resistivity because it affects the conduction of current. However, many soils have low natural conductivity, so how to improve the conductivity of grounded soil has become an urgent problem to be solved.
[0003] Bentonite, as a natural reinforcement material, has been widely used to improve the conductivity of grounded soil. Montmorillonite is one of the main components of bentonite and is a layered aluminum silicate non-metallic mineral with a "sandwich" structure. The basic unit cell of montmorillonite is a highly ordered crystal composed of two silicon-oxygen tetrahedrons above and below and an aluminum-oxygen octahedron in the middle. Montmorillonite has been widely studied and applied due to its unique interlayer structure and high cation exchange capacity. However, the application of sodium montmorillonite (Na-MMT) in improving soil conductivity is limited due to its relatively low conductivity.
[0004] In order to improve the performance of montmorillonite, people usually achieve this goal by modifying montmorillonite. Inorganic modified montmorillonite can significantly improve its physical and chemical properties by introducing different metal ions or inorganic compounds, making it have broad application prospects in the fields of environmental protection, energy materials, catalysts and composite materials. Zhu et al. (Microporous and Mesoporous Materials, 2006, 88 (1-3): 8-15.) synthesized iron-based montmorillonite by reacting montmorillonite with ferric nitrate hydrolysis solution. The modified montmorillonite can be used as an efficient catalyst and adsorbent. Wang et al. (Chemical engineering journal, 2010, 156 (1): 11-24.) modified sodium-based montmorillonite into calcium-based montmorillonite for wastewater treatment and heavy metal adsorption. By intercalating highly conductive metal ions, the ion conductivity of montmorillonite can be significantly improved, thereby improving its conductivity. Lithium ions (Li+) are ideal for modifying sodium-based montmorillonite due to their small radius, high conductivity and chemical stability. Summary of the invention
[0005] The present invention aims to improve the conductivity of grounded soil and provides a lithium-based montmorillonite inorganic modified material, a preparation method and application thereof in ion conduction technology.
[0006] The present invention uses a microwave-assisted ultrasonic method to intercalate anhydrous lithium chloride into the interlayer of sodium-based montmorillonite, thereby realizing inorganic modification of the sodium-based montmorillonite and obtaining lithium-based montmorillonite. The present invention synthesizes an inorganic modified lithium-based montmorillonite material by adjusting the mass ratio of montmorillonite and lithium chloride, and finds that when the mass ratio is 1:1, the modified material can significantly improve the original ionic conductivity of the sodium-based montmorillonite; by testing the ionic conductivity of the lithium-based montmorillonite modified material at different temperatures and humidities, it is found that the inorganically modified material exhibits typical temperature and humidity-dependent ionic conductivity, and the conductivity increases with increasing temperature and increases with increasing humidity.
[0007] The first object of the present invention is to provide a method for preparing a lithium-based montmorillonite inorganic modified material (Li-MMT), the steps of which are as follows:
[0008] (1) dissolving sodium montmorillonite (Na-MMT) and anhydrous lithium chloride in a mass ratio of 1:1 in deionized water;
[0009] (2) subjecting the solution obtained in step (1) to ultrasonic treatment at 20 to 40° C. and a microwave power of 1200 to 1800 W for 5 to 10 hours;
[0010] (3) allowing the solution obtained in step (2) to cool naturally by standing, and then centrifuging, and washing the centrifuged product 2 to 4 times with a mixed solution of deionized water and anhydrous ethanol (the volume ratio of deionized water to anhydrous ethanol is 1:0.8 to 1.2);
[0011] (4) Drying the product obtained in step (3) at a constant temperature of 70 to 90° C. to a constant weight, thereby obtaining the lithium-based montmorillonite inorganic modified material (Li-MMT).
[0012] The second object of the present invention is to provide a lithium-based montmorillonite inorganic modified material (Li-MMT), which is prepared by the above method.
[0013] The third object of the present invention is to provide the application of the above-mentioned lithium-based montmorillonite inorganic modified material (Li-MMT) in ion conduction technology.
[0014] Beneficial Effects
[0015] 1. The present invention can successfully modify sodium-based montmorillonite into lithium-based montmorillonite, and has the characteristics of simple and easy preparation method.
[0016] 2. By controlling the mass ratio of sodium montmorillonite and anhydrous lithium chloride, the appropriate doping ratio was found. When the mass ratio of Na-MMT and anhydrous LiCl was 1:1, the ionic conductivity of the obtained product was significantly improved, which was 2 times or even more than that of the original Na-MMT.
[0017] 3. The test results under different temperatures and humidities show that the inorganic modified ones exhibit typical temperature and humidity dependent ionic conductivity. The conductivity increases with increasing temperature and increases with increasing humidity. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is the PXRD diffraction pattern of Na-MMT and Li-MMT-3, Li-MMT-2, Li-MMT-1, Li-MMT-1 / 2 and Li-MMT-1 / 3 synthesized by the present invention.
[0019] Figure 2 It is the FT-IR chart of Na-MMT and Li-MMT-3, Li-MMT-2, Li-MMT-1, Li-MMT-1 / 2 and Li-MMT-1 / 3 synthesized by the present invention.
[0020] Figure 3 These are SEM images of Na-MMT and the synthetic products of the present invention, wherein Figure (a) is Na-MMT, Figure (b) is Li-MMT-3, Figure (c) is Li-MMT-2, Figure (d) is Li-MMT-1, Figure (e) is Li-MMT-1 / 2, and Figure (f) is Li-MMT-1 / 3.
[0021] Figure 4 Nyquist curves of Na-MMT and the synthetic products of the present invention changing with temperature at 50% RH, wherein Figure (a) is Na-MMT, Figure (b) is Li-MMT-3, (c) Li-MMT-2, Figure (d) is Li-MMT-1, Figure (e) is Li-MMT-1 / 2, and Figure (f) is Li-MMT-1 / 3.
[0022] Figure 5 Nyquist curves of Na-MMT and the synthetic products of the present invention changing with temperature at 40% RH, wherein Figure (a) is Na-MMT, Figure (b) is Li-MMT-3, (c) Li-MMT-2, Figure (d) is Li-MMT-1, Figure (e) is Li-MMT-1 / 2, and Figure (f) is Li-MMT-1 / 3.
[0023] Figure 6 These are the temperature-dependent ionic conductivity curves of Na-MMT and the synthetic products of the present invention, Na-MMT, Li-MMT-3, Li-MMT-2, Li-MMT-1, Li-MMT-1 / 2, and Li-MMT-1 / 3 at 50% RH (Figure a) and 40% RH (Figure b). DETAILED DESCRIPTION
[0024] Example 1
[0025] Preparation of lithium-based montmorillonite: Sodium-based montmorillonite is recorded as Na-MMT, and the lithium-based montmorillonite inorganic modified material is obtained according to the different masses of montmorillonite and anhydrous lithium chloride participating in the reaction. ag Na-MMT and bg anhydrous lithium chloride (x = a: b = 3: 1, 2: 1, 1: 1, 1: 2 and 1: 3, that is, the mass amounts of Na-MMT and anhydrous lithium chloride are 4.5g and 1.5g, 4g and 2g, 3g and 3g, 2g and 4g, 1.5g and 4.5g respectively) are dissolved in 400mL of deionized water, assisted by ultrasound at 30°C and 1500W microwave power for 8 hours, naturally cooled, centrifuged, and then washed with deionized water and The centrifuged products were washed three times with ethanol solution (volume ratio of 1:1) and dried in a constant temperature drying oven at 80°C to constant weight. The masses of the five products were 3.73g, 3.51g, 2.42g, 1.72g, and 1.32g, respectively, to obtain the lithium-based montmorillonite inorganic modified materials (Li-MMT-x, namely Li-MMT-3, Li-MMT-2, Li-MMT-1, Li-MMT-1 / 2, and Li-MMT-1 / 3, respectively).
[0026] Some basic characterizations were performed on the materials prepared by the above method.
[0027] Figure 1 Figure 2 shows the PXRD of montmorillonite before and after modification. The montmorillonite Na-MMT that has not been treated with lithium salt has a strong diffraction peak at 2θ=5.7°, while the 2θ angles of the modified Li-MMT-3, Li-MMT-2, Li-MMT-1, Li-MMT-1 / 2, and Li-MMT-1 / 3 shift to the right to 5.87°, 5.84°, 6.8°, 6.19°, and 6.15°, respectively; According to the Bragg equation: 2dsinθ=nλ, it is found that the interlayer spacing of Li-MMT is smaller than that of Na-MMT, which is due to the Li + The radius (0.76°A) is much smaller than Na + radius (1.02°A), indicating the deintercalation of Na ions and Li + intercalation effect.
[0028] Figure 2 FT-IR of montmorillonite before and after modification. In the high frequency region 3624cm -1 The infrared characteristic absorption peak is caused by the stretching vibration of the hydroxyl groups on the surface of montmorillonite, with a high frequency of 3431 cm -1 and the mid-frequency region 1642cm -1 The characteristic absorption peak at is caused by the stretching vibration of the hydroxyl group of water located between the montmorillonite layers. -1 The characteristic absorption peak of 458 cm represents the asymmetric stretching vibration of the tetrahedral Si-O-Si plane between the montmorillonite skeletons. -1and 521cm -1 The characteristic absorption peak at 903cm is caused by the bending vibration of Si-O-Al in tetrahedral Si-O-Si. -1 The OH vibration bands are attributed to the octahedral Al-O-Al between the montmorillonite skeleton. As can be seen from the figure, the characteristic peaks of the FT-IR spectra of the inorganically modified montmorillonite Li-MMT-x and the original Na-MMT are basically the same, which indicates that during the modification process, lithium ions did not have a significant effect on the structure of montmorillonite. Although lithium ions (Li + ) and sodium ions (Na + ) differ in charge and radius, but they are both alkali metal ions with similar chemical properties.
[0029] Figure 3 The SEM of montmorillonite before and after modification. The montmorillonite molecule is composed of two layers of Si-O tetrahedron and one layer of Al (or Mg)-O (or -OH) octahedron, such as Figure 3 The scanning electron microscope image shown in the figure shows that the inorganically modified Li-MMT-x retains the typical nanosheet structure of Na-MMT, indicating that the inorganic modification will not affect the morphology of the montmorillonite itself, and it still maintains the original morphology, indicating that its tetrahedral and octahedral sheet structures are stable.
[0030] The sample was ground into a uniform powder, placed in a mold with an inner diameter of 5 mm, pressed for 30 seconds under a pressure of 20 MPa, and the thickness was measured with a digital micrometer thickness gauge. The sample was sandwiched between two gold-plated electrodes, and the ionic conductivity of the synthesized material was measured using the alternating current (AC) impedance method of an impedance / gain phase analyzer under the conditions of controlling the temperature and relative humidity in a constant temperature and humidity experimental box. The test frequency range was 1 Hz to 1 MHz, and the applied voltage was 50 mV. For the variable temperature electrochemical impedance spectroscopy (EIS) test, thermal equilibrium was maintained for 60 minutes under each temperature condition, and the test temperature range was 20°C to 60°C. The Z' and Z" data obtained by Zview software were plotted as x, z, and y axes to obtain the 3D Nyquist curve of the material changing with temperature.
[0031] The formula for calculating proton conductivity (σ) using impedance value is:
[0032] σ=l / AR
[0033] Where: σ (S / cm) is the ionic conductivity; (l cm) is the thickness of the test sample slice; A (cm 2 ) is the area of the test sample slice; R (Ω) is the impedance of the test sample. The ionic conductivity of the material at different temperatures can be obtained by plotting Logσ as the ordinate and temperature as the abscissa.
[0034] An appropriate concentration of lithium chloride can effectively reduce the migration energy barrier of cations between montmorillonite layers, thereby improving the conductivity. Therefore, this application evaluates the ionic conductivity of the material before and after modification. In order to better apply it to daily life, AC impedance spectroscopy measurements were performed at 40% RH and 50% RH, 20-60°C. Figure 4 and Figure 5 It can be seen that the impedance value of the material decreases with increasing temperature, and the ionic conductivity increases with increasing temperature, indicating that the material shows typical temperature-dependent ionic conductivity, which is attributed to the acceleration of ion migration rate due to increased temperature. Figure 4 and Figure 5 It was found that as humidity increased, the impedance of the material decreased and the conductivity increased. This is because when lithium chloride is used for exchange, Li + Embedded in the interlayer space of montmorillonite to form Li-MMT. This shows that interlayer water can significantly improve the ion transfer rate and kinetic performance in MMT. Under high humidity conditions, the amount of interlayer water increases, and water molecules interact with Li through electrostatic interaction. + The formation of hydrated ions promotes the migration of ions between layers, and the conductivity is improved accordingly.
[0035] In order to find the appropriate doping ratio, ion conductivity tests were performed on materials with different doping ratios at 40% RH and 50% RH. Figure 6 It was found that when the mass ratio of sodium montmorillonite (Na-MMT) and anhydrous lithium chloride was 1:1, the conductivity of the material was higher than that of the original sodium montmorillonite. The ionic conductivity of Na-MMT at 50% RH and 60°C was 3.94×10 -4 S cm -1 The ionic conductivity of Li-MMT-1 is 6.3×10 -4 S cm -1 ; The ionic conductivity of Na-MMT at 40% RH and 60°C is 9.81×10 -5 S cm -1 The ionic conductivity of Li-MMT-1 is 4.15×10 -4 S cm -1 . Under other temperature conditions, the ionic conductivity of Li-MMT-1 is higher than that of Na-MMT under the same temperature conditions. Experiments show that when the concentration of lithium chloride is too high or too low, it will not effectively improve the ionic conductivity of montmorillonite. When the concentration is too low, its conductivity is poor due to insufficient number of ions. As the concentration increases, the number of these ions increases, thereby improving the conductivity of the solution. However, when the concentration increases to a certain level, although the number of dissociated ions increases, the interaction between ions is enhanced at the same time, and the ion conduction path is too crowded, resulting in a decrease in mobility and a decrease in conductivity.
Claims
1. A method for preparing a lithium-based montmorillonite inorganic modified material, comprising the following steps: (1) dissolving sodium montmorillonite and anhydrous lithium chloride in a mass ratio of 1:1 in deionized water; (2) subjecting the solution obtained in step (1) to ultrasonic treatment at 20 to 40° C. and a microwave power of 1200 to 1800 W for 5 to 10 hours; (3) allowing the solution obtained in step (2) to cool naturally, then centrifuging, and washing the centrifuged product with a mixed solution of deionized water and anhydrous ethanol; (4) Drying the product obtained in step (3) at a constant temperature of 70 to 90° C. to a constant weight, thereby obtaining the lithium-based montmorillonite inorganic modified material.
2. The method for preparing a lithium-based montmorillonite inorganic modified material according to claim 1, characterized in that: In step (3), washing is performed 2 to 4 times with a mixed solution of deionized water and anhydrous ethanol.
3. The method for preparing a lithium-based montmorillonite inorganic modified material according to claim 1, characterized in that: In step (3), the volume ratio of deionized water to anhydrous ethanol is 1:0.8-1.
2.
4. A lithium-based montmorillonite inorganic modified material, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 3.
5. Application of the lithium-based montmorillonite inorganic modified material according to claim 4 in ion conduction technology.
Citation Information
Patent Citations
Lithium-based montmorillonite @ sulfur composite material and preparation method and application thereof
CN109148841A
Method for modifying calcium bentonite
CN111470514A
Method for preparing sodium bentonite by using sodium fluoride through semi-dry method under assistance of microwaves
CN112694094A
Lithium montmorillonite, preparation method of lithium montmorillonite, composite solid electrolyte and application of composite solid electrolyte
CN115611290A
Preparation method of light and thin modified PE diaphragm with high mechanical strength and high lithium ion flux
CN117801346A