Preparation method and application of black cerium dioxide material
The black ceria material is prepared by contacting ceria powder with hydrogen, and using its color change characteristics, the high cost and complexity of oxygen detection are solved, and a low-cost and easy-to-operate oxygen detection method is provided. Suitable for chemical production and other fields.
Patent Information
- Application Number
- CN202310497656.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-05
- Publication Date
- 2024-11-05
AI Technical Summary
In the prior art, oxygen detection relies on expensive and complex instruments and lacks simple and economical detection methods. Especially in the fields of chemical production, food processing and microbial fermentation, a low-cost oxygen component detection method is needed.
By contacting the ceria powder with a reducing gas such as hydrogen, a black ceria material is prepared and oxygen detection is used to detect the color from black to white when oxygen is present, and an oxygen-free detection device is designed to observe the color of the material. change.
It realizes a low-cost and easy-to-operate oxygen detection method, with significant detection results. It is suitable for chemical production, food processing, and microbial fermentation and other fields, providing an economical and efficient oxygen detection solution.
Smart Images

Figure CN118894547A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a preparation method and application of a black cerium dioxide material, and belongs to the technical field related to material preparation. Background Art
[0002] my country has rich rare earth resources, accounting for 23% of the world's total proven rare earth reserves. Rare earth resources include scandium (Sc), yttrium (Y) and lanthanide elements, a total of 17 elements, among which cerium has the highest content. Cerium dioxide (CeO2), as the most common oxide carrier of cerium, has high hardness and stability and can be used as a polishing material. Microscopically, its crystals have a cubic fluorite structure with a space group of Fm3m. O ions are located in tetrahedral vacancies around Ce ions. When O atoms leave the crystal, oxygen vacancies can be formed, making it in an oxygen defect state.
[0003] The formation and disappearance of oxygen vacancies in CeO2 gives it the ability to store oxygen. When CeO2 is treated with reducing gas at high temperature, O atoms are removed and a large number of O vacancies are generated inside the crystal. When the crystal with oxygen vacancies is exposed to an oxygen atmosphere again, its surface can adsorb O2 molecules to supplement its own oxygen defects. This process can be cyclic. Therefore, CeO2 is used in the catalytic field, such as methanol reforming reaction, water gas change reaction, reduction reaction of nitrogen oxides, etc.
[0004] CeO2 has a light yellow appearance and strong ultraviolet absorption ability, and can be used in the field of photocatalysis. When CeO2 is reduced, the generation of oxygen vacancies in CeO2 causes the wavelength of its absorbed light to change, and the color changes from light yellow to blue or black. When exposed to air again, the oxygen vacancies are filled, and the color changes from black to white or grayish white. Wen and other researchers prepared a CeO2-Ag / AgBr composite catalyst. Under the initiation of visible light, the material can be used for the photocatalytic degradation of ciprofloxacin (CIP). When the initial concentration of CIP is 10 mg / L, the removal rate can reach 93% (Journal of Catalysis, 2018, 358, 141-154, org / 10.1016 / j.jcat.2017.11.029).
[0005] In addition, in some operating links in the fields of chemical production, material processing, microbial fermentation, etc., an oxygen-free environment is required. However, oxygen detection currently relies on oxygen detectors, which are costly and complex to operate. In actual production, a simpler and more economical detection method is needed. Relying on the color change effect of chemical substances on oxygen adsorption is an alternative method, and how to prepare such materials and apply them to the detection of oxygen components in the atmosphere is a technical problem that needs to be solved urgently. Summary of the invention
[0006] According to one aspect of the present application, a method for preparing a black cerium dioxide material is provided, the preparation method comprising:
[0007] contacting the cerium dioxide powder with a reducing gas for reduction treatment to obtain the black cerium dioxide material;
[0008] The temperature of the reduction treatment is 450-900° C., and the time of the reduction treatment is 0.5-10 hours.
[0009] The reducing gas is hydrogen.
[0010] Optionally, the temperature of the reduction treatment is selected from any value of 450°C, 480°C, 520°C, 580°C, 600°C, 700°C, 750°C, 800°C, 900°C or a range between any two of the above points.
[0011] Optionally, the reduction treatment time is selected from any value of 0.5h, 0.8h, 1h, 2h, 2.5h, 3h, 4h, 5h, 6h, 8h, 10h or a range between any two of the above points.
[0012] Optionally, the reduction treatment temperature is 480-580° C., and the reduction treatment time is 0.8-2.5 h.
[0013] Optionally, the reducing gas further includes an inert gas, and the inert gas is selected from at least one of nitrogen, argon, helium and carbon dioxide.
[0014] Optionally, the volume fraction of the hydrogen gas to the reducing gas is 15% to 100%.
[0015] Optionally, the volume fraction of the hydrogen in the reducing gas is selected from any value among 15%, 20%, 25%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 100% or a range between any two of the above points.
[0016] Optionally, the gas space velocity of the reducing gas is 2 to 30 L g -1 h -1 , the gas space velocity of the reducing gas is based on the mass of cerium dioxide.
[0017] Optionally, the gas space velocity of the reducing gas is selected from 2.0L g -1 h -1 , 3.0L g -1 h -1 , 5.0L g -1 h -1 , 7.0L g -1 h -1, 10L g -1 h -1 , 15L g -1 h -1 , 20L g -1 h -1 , 25L g -1 h -1 、30L g -1 h -1 Any value in or a range of values between any two of the above points.
[0018] Optionally, the gas space velocity of the reducing gas is 3.0 to 5.0 L g -1 h -1 , the gas space velocity of the reducing gas is based on the mass of cerium dioxide.
[0019] According to another aspect of the present application, there is provided an application of the black cerium dioxide material prepared by the preparation method described above in oxygen detection, wherein an oxygen-containing gas is introduced into an oxygen detection device filled with the black cerium dioxide material, and the color change of the cerium dioxide material in the oxygen detection device is observed;
[0020] The oxygen detection device is an anaerobic oxygen detection device.
[0021] Optionally, the volume fraction of oxygen in the oxygen-containing gas is 0.5% to 100%.
[0022] Optionally, the temperature at which the color of the black cerium dioxide material changes is 15°C to 150°C.
[0023] According to another aspect of the present application, there is provided an application of a black cerium dioxide material prepared by the preparation method described above in detection in the fields of chemical production, food processing, and microbial fermentation.
[0024] The beneficial effects of this application include:
[0025] 1) The raw materials of the black cerium dioxide prepared in this application are easily available, the preparation method is simple, the cost is low, and it has wide applicability and obvious effect in the detection of oxygen-containing gases. It has certain application prospects in the fields of chemical production and so on.
[0026] 2) The black cerium dioxide material prepared in this application has a solid appearance and black color at room temperature. When the material comes into contact with oxygen molecules, the appearance color gradually changes from black to white. When the amount of oxygen contact exceeds the saturated oxygen absorption of the material, the black solid will turn completely white. The color change process is highly recognizable, easy to observe with the naked eye, sensitive to oxygen response, and the material has low production cost and has application prospects in fields that require anaerobic conditions such as chemical production, food processing, and microbial fermentation. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is the XRD spectrum of the black cerium dioxide material in Example 1 of the present application.
[0028] Figure 2 This is a schematic diagram of the structure of the device for detecting oxygen-containing gas using black cerium dioxide material in Test Examples 1 to 3 of this application.
[0029] Figure 2 In the figure, 1. air inlet, 2. quartz tube, 3. temperature control furnace, 4. black cerium dioxide. DETAILED DESCRIPTION
[0030] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0031] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.
[0032] Commercial cerium dioxide was purchased from Sigma-Aldrich.
[0033] XRD was measured by an Empyrean X-ray diffractometer from Malvern Panalytical.
[0034] The “room temperature” in the embodiments of the present application refers to “25° C.”
[0035] The preparation method of black cerium dioxide used in this application comprises the following steps:
[0036] The commercial cerium dioxide is loaded into a fixed bed reactor, a reducing gas with a certain flow rate is introduced, and the reactor is heated for a certain period of time and cooled to room temperature to obtain a black cerium dioxide material.
[0037] The method for detecting oxygen using black cerium dioxide material in the present application comprises the following steps:
[0038] Black cerium dioxide material is filled in a transparent pipe. When oxygen-containing gas passes through, the black cerium dioxide can react with it, and the color gradually changes from black to white.
[0039] Example 1
[0040] Weigh 0.1 g of commercial cerium dioxide powder, load it into the tube of a fixed bed reactor, and introduce 10 mL / min of H2 (space velocity 6 L g -1 h -1 ), and then heated to 800°C at 10°C / min, and kept at this temperature for 0.5h, then stopped heating, and cooled to room temperature to obtain the desired black cerium dioxide material 1. Figure 1It can be seen that the strongest diffraction peak appears at the position where 2θ is equal to 28.5°, corresponding to the diffraction peak of the (111) crystal plane of CeO2. Then there are three obvious diffraction peaks located at 33.1, 47.5, and 56.3°, which correspond to the (200), (220), and (311) crystal planes of CeO2 respectively. The remaining diffraction peaks are also consistent with the standard card of CeO2 crystal, and no other diffraction peaks appear, indicating that the prepared material is indeed CeO2.
[0041] Example 2
[0042] Weigh 0.2 g of commercial cerium dioxide powder and load it into the tube of a fixed bed reactor. Pass 50 mL / min of a mixture of H2 and Ar (space velocity 15 L g -1 h -1 ), calculated by volume fraction, of which H2 accounts for 15% and Ar accounts for 85%, the temperature is raised to 700°C at 10°C / min and maintained at this temperature for 4 hours, then the heating is stopped and the temperature is cooled to room temperature to obtain the desired black cerium dioxide material 2.
[0043] Example 3
[0044] Weigh 0.1 g of commercial cerium dioxide powder and load it into the tube of a fixed bed reactor. Pass 15 mL / min of a mixture of H2 and He (space velocity 9 L g -1 h -1 ), calculated by volume fraction, of which H2 accounts for 50% and He accounts for 50%, the temperature is raised to 650°C at 10°C / min and maintained at this temperature for 5h, after which the heating is stopped and the temperature is cooled to room temperature to obtain the desired black cerium dioxide material 3.
[0045] Example 4
[0046] 0.3 g of commercial cerium dioxide powder was weighed and loaded into the tube of a fixed bed reactor. A mixture of H2 and Ar (space velocity 20 L g) was introduced at a flow rate of 100 mL / min. -1 h -1 ), calculated by volume fraction, wherein H2 accounts for 10% and Ar accounts for 90%, the temperature is raised to 900°C at 5°C / min and maintained at this temperature for 0.5h, then the heating is stopped and the temperature is cooled to room temperature to obtain the desired black cerium dioxide material 4.
[0047] Example 5
[0048] Weigh 0.05 g of commercial cerium dioxide powder and load it into the tube of a fixed bed reactor. Pass 25 mL / min of a mixture of H2 and carbon dioxide (space velocity 30 L g -1 h -1), calculated by volume fraction, of which H2 accounts for 40% and CO2 accounts for 60%, the temperature is raised to 500°C at 8°C / min and maintained at this temperature for 1 hour, then the heating is stopped and the temperature is cooled to room temperature to obtain the desired black cerium dioxide material 5.
[0049] Example 6
[0050] Weigh 0.3 g of commercial cerium dioxide powder and load it into the tube of a fixed bed reactor. Pass 25 mL / min of a mixture of H2 and nitrogen (space velocity 5 L g -1 h -1 ), calculated by volume fraction, of which H2 accounts for 40% and N2 accounts for 60%, the temperature is raised to 450°C at 8°C / min and maintained at this temperature for 10 hours, then the heating is stopped and the temperature is cooled to room temperature to obtain the desired black cerium dioxide material 6.
[0051] Comparative Example 1
[0052] Weigh 0.1 g of commercial cerium dioxide powder and load it into the tube of a fixed bed reactor. Pass 25 mL / min of a mixture of H2 and carbon dioxide (space velocity 15 L g -1 h -1 ), calculated by volume fraction, of which H2 accounted for 10% and CO2 accounted for 90%, and the temperature was raised to 400°C at 10°C / min and maintained at this temperature for 0.5h, after which the heating was stopped and the temperature was cooled to room temperature, and no black cerium dioxide was obtained.
[0053] Comparative Example 2
[0054] Weigh 0.2 g of commercial cerium dioxide powder, load it into the tube of a fixed bed reactor, and introduce 25 mL / min of N2 (space velocity 7.5 L g -1 h -1 ), the temperature was raised to 600°C at a rate of 10°C / min and maintained at this temperature for 2h, after which the heating was stopped and the temperature was cooled to room temperature. The color was still light yellow and no black cerium dioxide was obtained.
[0055] Test Example 1
[0056] 0.3 g of the black cerium dioxide material prepared in Example 5 was placed in Figure 2 The quartz tube 2 in the test device shown was evaluated for its ability to detect oxygen-containing gas. At an ambient temperature of 35°C in a temperature-controlled furnace 3, an O2-N2 mixed gas (O2 volume fraction of 1%) with a flow rate of 20 mL / min was introduced from the air inlet 1. The color of the top black cerium dioxide material changed within less than 20 seconds. As the oxygen-containing gas was gradually introduced, the appearance of the black cerium dioxide material gradually changed from black to white. After 5 minutes, it all turned white.
[0057] Test Example 2
[0058] 0.2 g of the black cerium dioxide material prepared in Example 5 was placed in Figure 2 The quartz tube 2 in the test device shown was evaluated for its ability to detect oxygen-containing gas. At an ambient temperature of 20°C in a temperature-controlled furnace 3, an O2-N2 mixed gas (O2 volume fraction of 1%) with a flow rate of 100 mL / min was introduced from the air inlet 1. Within 15 seconds, the color of the top black cerium dioxide material was observed to change. As the oxygen-containing gas was gradually introduced, the appearance of the black cerium dioxide material gradually changed from black to white. After 3 minutes, it turned completely white.
[0059] Test Example 3
[0060] 0.05 g of the black cerium dioxide material 3 prepared in Example 3 was placed in Figure 2 The quartz tube 2 in the test device shown was evaluated for its ability to detect oxygen-containing gas. At an ambient temperature of 150°C in a temperature-controlled furnace 3, an O2-N2 mixed gas (O2 volume fraction of 0.5%) with a flow rate of 50 mL / min was introduced from the air inlet 1. The color of the top black cerium dioxide material changed within less than 5 seconds. As the oxygen-containing gas was gradually introduced, the appearance of the black cerium dioxide material gradually changed from black to white, and after 1 minute, it all turned white.
[0061] The above are only a few embodiments of the present application and are not intended to limit the present application in any form. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the present profession, without departing from the scope of the technical solution of the present application, using the above disclosed technical content to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical DD230134I-DL solution.
Claims
1. A method for preparing a black cerium dioxide material, characterized in that: The preparation method comprises: The cerium dioxide powder is contacted with a reducing gas for reduction treatment to obtain the black cerium dioxide material; The temperature of the reduction treatment is 450-900° C., and the time of the reduction treatment is 0.5-10 hours. The reducing gas is hydrogen.
2. The preparation method according to claim 1, characterized in that: The temperature of the reduction treatment is 480-580° C., and the time of the reduction treatment is 0.8-2.5 h.
3. The preparation method according to claim 1, characterized in that: The reducing gas also includes an inert gas, and the inert gas is selected from at least one of nitrogen, argon, helium, and carbon dioxide.
4. The preparation method according to claim 3, characterized in that: The volume fraction of the hydrogen gas to the reducing gas is 15% to 100%.
5. The preparation method according to claim 1, characterized in that: The gas space velocity of the reducing gas is 2 to 30 Lg -1 h -1 , the gas space velocity of the reducing gas is based on the mass of cerium dioxide.
6. The preparation method according to claim 5, characterized in that: The gas space velocity of the reducing gas is 3.0 to 5.0 L g -1 h -1 , the gas space velocity of the reducing gas is based on the mass of cerium dioxide.
7. Application of the black cerium dioxide material prepared by the preparation method according to any one of claims 1 to 6 in oxygen detection, characterized in that: Passing oxygen-containing gas into an oxygen detection device filled with black cerium dioxide material, and observing the color change of the black cerium dioxide material in the oxygen detection device; The oxygen detection device is an anaerobic oxygen detection device.
8. The use according to claim 7, characterized in that: The volume fraction of oxygen in the oxygen-containing gas is 0.5% to 100%.
9. The use according to claim 7, characterized in that: The temperature at which the black cerium dioxide material changes color is 15°C to 150°C.
10. Application of the black cerium dioxide material prepared by the preparation method according to any one of claims 1 to 6 in detection in the fields of chemical production, food processing and microbial fermentation.