Capacitive deionization electrode, preparation method thereof and capacitive deionization device

By forming an ionomer coating that reacts with halogen-containing polymers and organic amines on the carbon material layer of the capacitor deionized electrode, the same-ion effect and scaling problems in CDI technology are solved, and the cycle life and deionization efficiency of the electrode are improved. , reduces production costs and resistance.

CN118894577APending Publication Date: 2024-11-05FOSHAN SHUNDE MIDEA WATER DISPENSER MFG +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411274337.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

In CDI technology, there are low charging efficiency and salt adsorption capacity caused by homo-ion effects and Faraday reactions, as well as electrode scaling problems, which affect deionization performance and life, and traditional ion exchange membranes increase resistance and cost.

Method used

Using a laminated structure, the capacitive deionized electrode is coated with halogen-containing polymer and organic amine on the carbon material layer to form an ionomer coating through in-situ quaternization reaction, improve cation adsorption performance, inhibit homo-ion effects and scaling, and reduce Resistance and production costs.

Benefits of technology

It significantly improves the cycle life and ion removal rate of the electrode, reduces the scaling and resistance of the electrode surface, and improves the performance and production efficiency of capacitor deionized devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894577A_ABST
    Figure CN118894577A_ABST
Patent Text Reader

Abstract

The invention provides a capacitive deionization electrode, a preparation method thereof and a capacitive deionization device. The capacitive deionization electrode comprises a current collector and a carbon material layer which are stacked, an ionomer coating is stacked on the side, away from the current collector, of the carbon material layer, the ionomer coating is obtained through an in-situ quaternization reaction of a halogen-containing polymer and organic amine, the halogen-containing polymer contains an aromatic ring, and the organic amine contains an aromatic ring. Halogen is connected to the aromatic ring or halogenated alkyl is connected to the aromatic ring. The capacitive deionization electrode has the advantages of higher ion removal rate, longer cycle life and lower manufacturing cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of water treatment, and in particular to a capacitor deionization electrode and a preparation method thereof, and a capacitor deionization device. Background Art

[0002] Capacitive deionization (CDI) is a technology that uses charge adsorption to remove ions from water. The core of CDI technology is a capacitor, which consists of two electrodes and a dielectric in the middle. In a CDI capacitor, when an external voltage is applied to the electrodes, an electric field is formed on the electrode surface, attracting ions to adsorb on the electrode surface. When the voltage disappears, the charge on the electrode surface disappears, and the ions are desorbed and enter the dielectric. Because the dielectric has a porous structure, it can increase the surface area and deionization efficiency of the capacitor. The advantages of CDI technology are that it does not require chemical reagents, does not generate waste, and does not pollute the environment.

[0003] CDI is based on ion adsorption through highly porous carbon electrodes with the electrical double layer (EDL) theory. When counter ions enter or expel auxiliary ions from the electrode, the entire charging process will generate current. Common ions refer to ions that have the same electrical properties as the electrode when charged, while counter ions have the opposite. However, only counter ion adsorption constitutes the theoretical current required for desalination. The current generated by excluding common ions is an additional current, which leads to unnecessary power and energy consumption. The "common ion effect" has been shown to reduce charging efficiency and salt adsorption capacity (SAC).

[0004] In addition to the common ion effect, another unavoidable problem of CDI is the Faraday reaction, namely carbon oxidation at the anode and oxygen reduction at the cathode, which leads to low charging efficiency and SAC, as well as the performance degradation of CDI electrodes during long-term desalination. At the cathode, the oxygen dissolved in the water undergoes a reduction reaction to generate hydrogen peroxide. Hydrogen peroxide further oxidizes the electrode, causing the electrode's desalination performance to deteriorate.

[0005] Another problem is scaling. Due to the influence of factors such as water quality and operating conditions, scaling will occur on the electrode surface. Electrode scaling refers to the formation of a thick layer of sediment on the electrode surface, which affects the deionization performance and life of the electrode. The main reason for electrode scaling is that dissolved substances in the water are adsorbed and deposited on the electrode surface to form sediments. The degree of electrode scaling is related to factors such as water quality, operating conditions, and electrode materials. Electrode scaling will affect the deionization performance and life of the electrode. First, electrode scaling will reduce the specific surface area and pore volume of the electrode, reduce the adsorption and desorption of ions on the electrode surface, and thus reduce the deionization efficiency of the electrode. Secondly, electrode scaling will increase the resistance of the electrode, reduce the capacitance of the capacitor, and increase the charging time of the capacitor, thereby reducing the deionization rate of the capacitor. Finally, electrode scaling will cause corrosion and wear on the electrode surface and shorten the service life of the electrode.

[0006] In order to solve the above problems, it is common practice to place a separate anion exchange membrane AEM on the CDI anode surface, or a separate cation exchange membrane CEM on the CDI cathode surface. However, the ion exchange membrane brings various resistances, such as the internal resistance and interface resistance of the membrane, and the large contact resistance between the membrane and the carbon electrode. In addition, the ion exchange membrane is expensive and the installation process is complicated, which limits its wide application. Summary of the invention

[0007] The present invention aims to solve one of the technical problems in the prior art at least to a certain extent. To this end, one object of the present invention is to provide a capacitor deionization electrode and a preparation method thereof and a capacitor deionization device.

[0008] In a first aspect of the present invention, the present invention provides a capacitor deionization electrode. According to an embodiment of the present invention, the capacitor deionization electrode comprises a stacked current collector and a carbon material layer, an ionomer coating is stacked on a side of the carbon material layer away from the current collector, the ionomer coating is obtained by an in-situ quaternization reaction of a halogen-containing polymer and an organic amine, the halogen-containing polymer contains an aromatic ring, a halogen is connected to the aromatic ring, or a halogenated alkyl is connected to the aromatic ring.

[0009] According to the capacitor deionization electrode of the above embodiment of the present invention, an ionomer coating is stacked on the carbon material layer, and the ionomer coating is obtained by in-situ quaternization reaction of a halogen-containing polymer and an organic amine, and the halogen-containing polymer contains an aromatic ring, and a halogen is connected to the aromatic ring or a halogenated alkyl is connected to the aromatic ring. The halogen in the halogen-containing polymer is more likely to undergo quaternization reaction with the organic amine, and the film layer obtained after the reaction carries a large amount of cations, which can have good adsorption properties for anions, can not only improve the ion removal rate, but also inhibit the common ion effect, reduce the deposition of scaling on the electrode surface, thereby significantly improving the cycle life of the electrode. Compared with the traditional separately arranged exchange membrane, the present application directly stacks the ionomer coating on the surface of the carbon material layer, and the carbon material layer has good interface contact with the ionomer coating, so as to have a lower resistance. On the other hand, compared with a separate exchange membrane, the preparation cost of the ionomer coating of the present application is lower, and the operation is simpler and more convenient, thereby significantly reducing the production cost.

[0010] In addition, the capacitive deionization electrode according to the above embodiment of the present invention also has the following technical features: In some embodiments of the present invention, the carbon number of the halogenated alkyl group is not greater than 12.

[0011] In some embodiments of the present invention, the halogen-containing polymer includes at least one of brominated polyphenylene ether, chlorinated polyphenylene ether, polyvinyl benzyl bromide, polyvinyl benzyl chloride, brominated styrene polymer, chlorinated styrene polymer, brominated polyetheretherketone, chlorinated polyetheretherketone, brominated ethylene terephthalate, and chlorinated ethylene terephthalate. Thus, the ion removal rate and cycle life of the electrode are improved.

[0012] In some embodiments of the present invention, the organic amine includes at least one of a primary amine, a secondary amine, a tertiary amine, and an imidazole compound.

[0013] In some embodiments of the present invention, the primary amine includes at least one of methylamine, ethylamine, and propylamine.

[0014] In some embodiments of the present invention, the secondary amine includes at least one of dimethylamine, diethylamine, and dipropylamine.

[0015] In some embodiments of the present invention, the tertiary amine includes at least one of trimethylamine, triethylamine, tert-butylamine, methyldiethanolamine, and diethylaminoethanol.

[0016] In some embodiments of the present invention, the imidazole compound includes at least one of 1-methylimidazole, 1-ethylimidazole, 1-propylimidazole, 1-phenylimidazole, 2-methylimidazole, and 2-ethylimidazole.

[0017] In some embodiments of the present invention, the thickness of the ionomer coating is 1-100 μm, thereby improving the ion removal rate and cycle life of the electrode.

[0018] In a second aspect of the present invention, the present invention provides a method for preparing the above-mentioned capacitor deionization electrode. According to an embodiment of the present invention, the method comprises: (1) dissolving a halogen-containing polymer in a solvent to obtain a halogen-containing polymer solution; (2) applying the halogen-containing polymer solution onto the carbon material layer and then drying it to obtain a precursor electrode; (3) Immersing the precursor electrode in an organic amine solution to undergo an in-situ quaternization reaction to obtain a capacitive deionization electrode.

[0019] According to the method for preparing a capacitor deionization electrode according to the above embodiment of the present invention, a halogen-containing polymer solution is applied to a carbon material layer and then dried to obtain a precursor electrode, and then the precursor electrode is immersed in an organic amine solution to undergo an in-situ quaternization reaction, and the halogen in the halogen-containing polymer and the organic amine fully undergo a quaternization reaction, thereby forming an ionomer coating with good contact on the surface of the carbon material layer, reducing internal resistance and electrode scaling, and improving the ion removal rate and cycle life of the electrode. The method has a simple process, low equipment investment, environmental safety, and low cost.

[0020] In addition, the method for preparing a capacitor deionization electrode according to the present invention also has the following technical features: In some embodiments of the present invention, in step (1), the mass concentration of the halogen-containing polymer in the halogen-containing polymer solution is 1% to 40%.

[0021] In some embodiments of the present invention, in step (2), the drying temperature is 60° C. to 120° C., and the drying time is 2 h to 30 h.

[0022] In some embodiments of the present invention, in step (3), the temperature of the in-situ quaternization reaction is 25°C to 100°C and the time is 2h to 48h, thereby increasing the degree of quaternization reaction and the number of cations on the surface of the ionomer coating.

[0023] In some embodiments of the present invention, in step (3), the concentration of the organic amine in the organic amine solution is 0.01 mol / L to 5 mol / L, thereby promoting the smooth progress of the quaternization reaction.

[0024] In some embodiments of the present invention, in step (3), the solvent used in the organic amine solution is water, thereby avoiding the use of organic solvents, which is more environmentally friendly and safe.

[0025] In a third aspect of the present invention, a capacitor deionization device is provided. According to an embodiment of the present invention, the capacitor deionization device comprises the above-mentioned capacitor deionization electrode or the capacitor deionization electrode prepared by the above-mentioned method. Thus, the capacitor deionization device has a higher ion removal rate, a longer cycle life and a lower production cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 is a schematic diagram of the structure of a capacitor deionization electrode according to an embodiment of the present invention; Figure 2 This is a schematic diagram of a quaternization reaction between a halogen polymer and an organic amine according to an embodiment of the present invention; Figure 3 is an electron microscope image of the ionomer coating of Example 1 of the present invention; Figure 4 This is an electron microscope image of the ionomer coating of Example 3 of the present invention. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] In a first aspect of the present invention, the present invention provides a capacitor deionization electrode. According to an embodiment of the present invention, reference is made to Figure 1 The capacitor deionization electrode includes a stacked current collector 100 and a carbon material layer 200, and an ionomer coating 300 is stacked on the side of the carbon material layer 200 away from the current collector 100. The ionomer coating 300 is obtained by an in-situ quaternization reaction of a halogen-containing polymer and an organic amine. The halogen-containing polymer contains an aromatic ring, and a halogen is connected to the aromatic ring or a halogenated alkyl is connected to the aromatic ring.

[0030] According to the capacitor deionization electrode of the above embodiment of the present invention, an ionomer coating 300 is stacked on the carbon material layer 200, and the ionomer coating 300 is obtained by an in-situ quaternization reaction of a halogen-containing polymer and an organic amine, and the halogen-containing polymer contains an aromatic ring, and a halogen is connected to the aromatic ring or a halogenated alkyl is connected to the aromatic ring. The halogen in the halogen-containing polymer is more likely to undergo a quaternization reaction with the organic amine, and the film layer obtained after the reaction carries a large amount of cations, which can have good adsorption properties for anions, can not only improve the ion removal rate, but also inhibit the common ion effect, reduce the deposition of scaling on the electrode surface, thereby significantly improving the cycle life of the electrode. Compared with the traditional separately arranged exchange membrane, the present application directly stacks the ionomer coating 300 on the surface of the carbon material layer 200, and the carbon material layer 200 has a good interface contact with the ionomer coating 300, so as to have a lower resistance. On the other hand, compared with a separate exchange membrane, the preparation cost of the ionomer coating of the present application is lower, and the operation is simpler and more convenient, thereby significantly reducing the production cost.

[0031] It should be noted that the current collector is a conventional material in the art, and those skilled in the art can select it according to actual conditions. For example, the current collector includes but is not limited to copper foil, aluminum foil, stainless steel foil, titanium foil, nickel foil, etc.

[0032] According to an embodiment of the present invention, the carbon material layer further includes a conductive agent and a binder. The conductive agent and the binder are conventional materials in the art, and those skilled in the art can select them according to actual conditions. For example, the conductive agent includes but is not limited to acetylene black, conductive carbon black, graphite powder, etc. The binder includes but is not limited to polyurethane, polystyrene, polyacrylate, polytetrafluoroethylene, etc.

[0033] According to an embodiment of the present invention, the carbon number of the halogenated alkyl group is not more than 12. For example, the carbon number is 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12. By controlling the carbon number to be not more than 12, it is beneficial for the halogen in the halogen-containing polymer to undergo a quaternization reaction with the organic amine.

[0034] According to an embodiment of the present invention, the halogen-containing polymer includes at least one of brominated polyphenylene ether, chlorinated polyphenylene ether, polyvinyl benzyl bromide, polyvinyl benzyl chloride, brominated styrene polymer, chlorinated styrene polymer, brominated polyetheretherketone, chlorinated polyetheretherketone, brominated ethylene terephthalate, and chlorinated ethylene terephthalate. The inventors have found that the halogen-containing polymer of the above structure is more likely to undergo quaternization reaction with organic amines, and the formed ionomer coating has more cations, thereby improving the ion removal rate and cycle life of the electrode.

[0035] According to an embodiment of the present invention, the organic amine includes at least one of a primary amine, a secondary amine, a tertiary amine, and an imidazole compound.

[0036] As an example, the primary amine includes but is not limited to at least one of methylamine, ethylamine, and propylamine.

[0037] As an example, the secondary amine includes but is not limited to at least one of dimethylamine, diethylamine, and dipropylamine.

[0038] As an example, the tertiary amine includes but is not limited to at least one of trimethylamine, triethylamine, tert-butylamine, methyldiethanolamine, and diethylaminoethanol.

[0039] As an example, the imidazole compound includes but is not limited to at least one of 1-methylimidazole, 1-ethylimidazole, 1-propylimidazole, 1-phenylimidazole, 2-methylimidazole, and 2-ethylimidazole.

[0040] According to an embodiment of the present invention, the thickness of the ionomer coating is 1-100 μm. For example, the thickness of the ionomer coating is 1 μm, 5 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, etc., and the thickness is greater than or equal to 1 μm, 5 μm, 10 μm, 20 μm, 30 μm, 40 μm, etc., and less than or equal to 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, etc. The inventors have found that controlling the thickness of the ionomer coating within the range of 1-100 μm can improve the desalination performance of the electrode.

[0041] In a second aspect of the present invention, the present invention provides a method for preparing the above-mentioned capacitor deionization electrode. According to an embodiment of the present invention, the method comprises: S100: Dissolving halogen-containing polymers in solvents

[0042] In this step, the halogen-containing polymer is dissolved in a solvent to obtain a halogen-containing polymer solution. Further, the solvent includes but is not limited to NMP, DMF, DMSO and the like.

[0043] According to an embodiment of the present invention, the mass concentration of the halogen-containing polymer in the halogen-containing polymer solution is 1% to 40%. For example, the concentration is 1%, 5%, 10%, 15%, 20%, 25%, 30%, 40%, etc., and the concentration is greater than or equal to 1%, 5%, 10%, 15%, etc., and less than or equal to 20%, 25%, 30%, 40%, etc. When the mass concentration of the halogen-containing polymer is controlled within the range of 1% to 40%, it is easier to apply it on the carbon material layer.

[0044] S200: Applying the halogen-containing polymer solution onto the carbon material layer and then drying

[0045] In this step, the halogen-containing polymer solution is applied to the carbon material layer and then dried to obtain a precursor electrode. The halogen-containing polymer solution is applied to the carbon material layer, and can fully wet and contact with the carbon material layer to reduce the contact resistance between the two. It should be noted that the above-mentioned application method is a conventional method in the art. For example, the application method includes but is not limited to roller coating, film pressing, brush coating, dip coating, spray coating, spin coating, electrospinning, etc. Further, the coating thickness of the halogen-containing polymer solution applied to the carbon material layer is 1μm~100μm. For example, the thickness is greater than or equal to 1μm, 5μm, 10μm, 20μm, 30μm, 40μm, etc., and less than or equal to 50μm, 60μm, 70μm, 80μm, 90μm, 100μm, etc.

[0046] According to an embodiment of the present invention, the drying temperature is 60°C to 120°C, for example, the temperature is greater than or equal to 60°C, 70°C, 80°C, etc., and less than or equal to 90°C, 100°C, 120°C, etc.; the drying time is 2h to 30h, for example, the time is greater than or equal to 2h, 5h, 10h, etc., and less than or equal to 15h, 20h, 30h, etc. By controlling the drying temperature to 60°C to 120°C and the time to 2h to 30h, the solvent can be effectively removed.

[0047] S300: Immerse the precursor electrode in an organic amine solution to undergo an in-situ quaternization reaction

[0048] In this step, refer to Figure 2 The precursor electrode is immersed in an organic amine solution to undergo an in-situ quaternization reaction, so that the halogen and organic amine in the halogen-containing polymer are fully quaternized, thereby forming an ionomer coating with good contact on the surface of the carbon material layer, reducing internal resistance and electrode scaling, and improving the ion removal rate and cycle life of the electrode.

[0049] According to an embodiment of the present invention, the temperature of the in-situ quaternization reaction is 25°C to 100°C, and the time is 2h to 48h. For example, the temperature is 25°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, etc., and the temperature is greater than or equal to 25°C, 30°C, 40°C, 50°C, etc., and less than or equal to 60°C, 70°C, 80°C, 90°C, 100°C, etc.; for example, the time is 2h, 5h, 10h, 20h, 30h, 40h, 48h, etc., and the time is greater than or equal to 2h, 5h, 10h, etc., and less than or equal to 20h, 30h, 40h, 48h, etc. By controlling the reaction temperature to 25°C to 100°C and the time to 2h to 48h, the degree of quaternization reaction can be increased, and the number of cations on the surface of the ionomer coating can be increased.

[0050] According to an embodiment of the present invention, the concentration of amine in the organic amine solution is 0.01mol / L to 5mol / L. For example, the concentration is 0.01mol / L, 0.1mol / L, 1mol / L, 2mol / L, 3mol / L, 4mol / L, 5mol / L, etc. For another example, the concentration is greater than or equal to 0.01mol / L, 0.1mol / L, 1mol / L, etc., and less than or equal to 2mol / L, 3mol / L, 4mol / L, 5mol / L, etc. Thus, the quaternization reaction is smoothly carried out.

[0051] According to an embodiment of the present invention, the solvent used in the organic amine solution is water, thereby avoiding the use of organic solvents, which is more environmentally friendly and safe.

[0052] In the third aspect of the present invention, the present invention proposes a capacitor deionization device. According to an embodiment of the present invention, the capacitor deionization device includes the above-mentioned capacitor deionization electrode or the capacitor deionization electrode prepared by the above-mentioned method. As a result, the capacitor deionization device has a higher ion removal rate, a longer cycle life and a lower production cost. It should be noted that the features and advantages described above for the capacitor deionization electrode and its preparation method are also applicable to the capacitor deionization device, and will not be repeated here.

[0053] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased through regular channels.

[0054] Example 1

[0055] (1) Preparation of anode electrode

[0056] (a) A carbon material slurry (slurry composition: 85 parts by weight of activated carbon, 8 parts by weight of conductive agent, 7 parts by weight of binder, 30% solid content of slurry) was scraped onto the current collector, dried at 80°C for 4 h, and rolled using a 90T roller press to form an electrode with a coating thickness of 80 μm.

[0057] (b) Preparation of halogen-containing polymer brominated polyphenylene ether: Dissolve 12 g of poly (2,6-dimethyl-1,4-phenylene ether) PPO in 100 mL of chlorobenzene, add 12 g of N-bromosuccinimide (NBS) and 0.6 g of azobisisobutyronitrile (AIBN). Heat to 135oC and reflux for 4 h. After cooling, slowly pour the reaction solution into 1 L of methanol under stirring to precipitate. Filter to obtain a pale yellow crude product. Dissolve the crude product in 100 mL of chlorobenzene, precipitate and purify in methanol. After filtering, dry the product BrPPO in an oven at 80°C for 8 h.

[0058] (c) Dissolving brominated polyphenylene ether BrPPO in NMP solvent to prepare a solution with a mass concentration of 10%, then applying the solution to the activated carbon electrode prepared in step (a), and then drying the electrode in an oven at 80° C. for 24 hours to prepare a precursor electrode.

[0059] (d) The precursor electrode was immersed in a 1 mol / L trimethylamine aqueous solution, reacted at room temperature for 24 hours, and then washed with clean water 5 times to prepare an anode electrode with an anion exchange membrane (ionomer coating). The specific reaction is as follows: The electron microscope image of the prepared anion exchange membrane shows Figure 3 ,from Figure 3 It can be seen that the thickness of the anion exchange membrane is about 2~3μm.

[0060] (2) Preparation of cathode electrode: Scrape carbon material slurry (slurry composition: 85 parts by weight of activated carbon, 8 parts by weight of conductive agent, 7 parts by weight of binder, 30% solid content of slurry) on the current collector, dry at 80°C for 4 h, and roll using a 90T roller press to form an electrode with a coating thickness of 80 um.

[0061] (3) Preparation of a capacitor deionization device: Alternately arrange capacitor deionization cathode electrode-spacer-capacitor deionization anode electrode-spacer to prepare a rolled capacitor deionization device.

[0062] Example 2

[0063] The difference between Example 2 and Example 1 is: (d) The precursor electrode was immersed in a 1 mol / L 1-methylimidazole aqueous solution and reacted at 60° C. for 24 hours. The electrode was then washed three times with clean water to prepare an anode electrode with an anion exchange membrane (ionomer coating).

[0064] Example 3

[0065] The difference between Example 3 and Example 1 is that on the basis of Example 1, a 10% concentration BrPPO solution is applied twice.

[0066] Step (1) Dissolve brominated polyphenylene ether BrPPO in NMP solvent to prepare a solution with a mass concentration of 10%, and then apply the solution to the activated carbon electrode prepared in step (1) a of Example 1, and then place the electrode in an oven at 80° C. to dry for 24 hours to prepare a precursor electrode. Then apply 10% BrPPO solution again, and after drying, obtain a precursor electrode.

[0067] Step (2) Immerse the above precursor electrode in a 1 mol / L trimethylamine aqueous solution, react at room temperature for 24 hours, and then wash the electrode 5 times with clean water to prepare an anode electrode with an anion exchange membrane (ionomer coating). The electron microscope image of the prepared anion exchange membrane shows Figure 4 ,from Figure 4 It can be seen that the thickness of the anion exchange membrane is about 3~5μm

[0068] Example 4

[0069] The difference between Example 4 and Example 2 is that the above-mentioned precursor electrode is immersed in a 1 mol / L diethylaminoethanol aqueous solution, reacted at 60° C. for 24 hours, and then washed with clean water three times to prepare an anode electrode with an anion exchange membrane (ionomer coating).

[0070] Comparative Example 1

[0071] (1) Preparation of anode electrode

[0072] Carbon material slurry (slurry composition: 85 parts by weight of activated carbon, 8 parts by weight of conductive agent, 7 parts by weight of binder, 30% solid content of slurry) was scraped on the current collector, dried at 80°C for 4 hours, and rolled using a 90T roller press to form an electrode with a coating thickness of 80um.

[0073] (2) Preparation of cathode electrode

[0074] Carbon material slurry (slurry composition: 85 parts by weight of activated carbon, 8 parts by weight of conductive agent, 7 parts by weight of binder, 30% solid content of slurry) was scraped on the current collector, dried at 80°C for 4 hours, and rolled using a 90T roller press to form an electrode with a coating thickness of 80um.

[0075] (3) Preparation of capacitive deionization devices

[0076] The preparation method of the capacitor deionization device in comparative example 1 is the same as that in example 1.

[0077] The performance of the capacitive deionization devices prepared in Examples 1-8 and Comparative Examples 1-2 was measured, as follows: Initial desalination rate (%): The electrodes prepared in Examples 1-4 and the electrodes of the comparative example are assembled into CDI devices according to the requirements of the positive and negative electrodes, and then the desalination test is carried out. The test conditions are as follows: the electrode area is 9cm x 9cm, the brine is prepared according to the GB34914-2021 reverse osmosis water efficiency standard, the starting point is 200TDS, the flow rate is 12mL / min, the adsorption voltage is 1.5V, the adsorption time is 150s, the desorption voltage is -1.5V, the desorption time is 100s, and the operation mode adopts Flow by Mode. The concentration change of the entire adsorption-desorption process is monitored in real time by a conductivity meter. Through the conversion relationship between solution concentration and conductivity, the concentration change before and after desalination can be obtained, and then the desalination rate of the device can be obtained.

[0078] Initial desalination rate (%): The desalination rate when the device starts to operate.

[0079] Salt removal rate after 100 cycles (%): Salt removal rate of the test device after 100 cycles.

[0080] The test results of the performance of the capacitive deionization devices prepared in Examples 1-8 and Comparative Examples 1-2 are shown in Table 1.

[0081] Table 1

[0082] As can be seen from Table 1, the electrode prepared by the present invention has a long cycle life. In Comparative Example 1, the anode was not modified by the polymer, and the salt rejection rate of the electrode decreased by 10.6% after 100 cycles, while in Examples 1-4 of the present application, the salt rejection rate decreased by no more than 2% after 100 cycles. Compared with Comparative Example 1, the initial salt rejection rate of Examples 1-4 was also improved to a certain extent.

[0083] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A capacitive deionization electrode, characterized in that: The capacitor deionization electrode comprises a stacked current collector and a carbon material layer, wherein an ionomer coating is stacked on a side of the carbon material layer away from the current collector, wherein the ionomer coating is obtained by an in-situ quaternization reaction of a halogen-containing polymer and an organic amine, wherein the halogen-containing polymer contains an aromatic ring, and a halogen is connected to the aromatic ring or a halogenated alkyl is connected to the aromatic ring.

2. The electrode according to claim 1, characterized in that: The carbon number of the haloalkyl group is not greater than 12; And / or, the halogen-containing polymer includes at least one of brominated polyphenylene ether, chlorinated polyphenylene ether, polyvinyl benzyl bromide, polyvinyl benzyl chloride, brominated styrene polymer, chlorinated styrene polymer, brominated polyetheretherketone, chlorinated polyetheretherketone, brominated polyethylene terephthalate, and chlorinated polyethylene terephthalate.

3. The electrode according to claim 1, characterized in that: The organic amine includes at least one of primary amine, secondary amine, tertiary amine and imidazole compounds.

4. The electrode according to claim 3, characterized in that: The primary amine includes at least one of methylamine, ethylamine and propylamine; And / or, the secondary amine includes at least one of dimethylamine, diethylamine, and dipropylamine; And / or, the tertiary amine includes at least one of trimethylamine, triethylamine, tert-butylamine, methyldiethanolamine, and diethylaminoethanol; And / or, the imidazole compound includes at least one of 1-methylimidazole, 1-ethylimidazole, 1-propylimidazole, 1-phenylimidazole, 2-methylimidazole, and 2-ethylimidazole.

5. The electrode according to any one of claims 1 to 4, characterized in that: The thickness of the ionomer coating is 1-100 μm.

6. A method for preparing the capacitive deionization electrode according to any one of claims 1 to 5, characterized in that: include: (1) dissolving a halogen-containing polymer in a solvent to obtain a halogen-containing polymer solution; (2) applying the halogen-containing polymer solution onto the carbon material layer and then drying it to obtain a precursor electrode; (3) Immersing the precursor electrode in an organic amine solution to undergo an in-situ quaternization reaction to obtain a capacitive deionization electrode.

7. The method according to claim 6, characterized in that: In step (1), the mass concentration of the halogen-containing polymer in the halogen-containing polymer solution is 1% to 40%.

8. The method according to claim 6, characterized in that: In step (2), the drying temperature is 60°C to 120°C, and the drying time is 2h to 30h.

9. The method according to claim 6, characterized in that: In step (3), the temperature of the in-situ quaternization reaction is 25°C to 100°C, and the time is 2h to 48h; And / or, the concentration of amine in the organic amine solution is 0.01 mol / L to 5 mol / L; And / or, the solvent used in the organic amine solution is water.

10. A capacitive deionization device, characterized in that: The invention comprises the capacitive deionization electrode as described in any one of claims 1 to 5 or the capacitive deionization electrode prepared by the method as described in any one of claims 6 to 9.

Citation Information

Patent Citations

  • Preparation method of crosslinking type polymer anion exchange membrane

    CN103159974A

  • Capacitive deionization electrode, preparation method thereof and capacitive deionization device

    CN111484105A

  • Process for electrolytically applying polymer coatings on electroconductive articles

    GB1401792A

  • Method for forming multilayer coating film

    JP2008229433A

  • Methods of manufacture of ion exchange membranes

    US20240033689A1