Non-pressure type constraint sintering method of LTCC (Low Temperature Co-Fired Ceramic) substrate
By setting up forced pressing plates and non-contact restraining plates on the LTCC substrate, the warping problem during sintering is solved by using the coordination of follow-up support blocks and restraining plates, and the flatness of the substrate is improved. It is suitable for most commercial LTCC materials. Achieve high flatness sintering effect.
Patent Information
- Application Number
- CN202410928733.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-05
AI Technical Summary
Existing LTCC substrates are prone to warping during sintering, resulting in low flatness, limiting the flexibility of circuit design and process design, and common constraint sintering methods are not compatible with most commercial LTCC materials.
By using the pressure-free constrained sintering method, the forced compression sheet and the non-contact constrained pressure plate are provided on the surface of the raw porcelain embryo, the relative position and material differences between the follow-up support block and the constrained pressure plate are used to improve the flatness of the substrate and reduce the Warpage during sintering.
Without changing the circuit design and sintering conditions, the final flatness of the LTCC substrate is effectively improved and the warpage during sintering is reduced. It is suitable for most commercial LTCC materials.
Smart Images

Figure CN118894729A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of LTCC circuit substrate manufacturing, in particular to a pressureless restraint sintering method for an LTCC substrate. Background Art
[0002] LTCC (low temperature co-fired ceramic) has the characteristics of high density integration, good airtight packaging characteristics, and excellent high-frequency performance, and is widely used in the field of microwave / millimeter wave communications. However, as the product form changes from traditional MCM hybrid integration to SIP integration, the LTCC substrate needs to act as an airtight packaging carrier while realizing circuit interconnection. It is necessary to perform airtight frame welding on the surface of the LTCC substrate and perform BGA surface mounting on the back of the LTCC substrate. Therefore, the LTCC substrate needs to have a higher flatness to achieve a good assembly effect.
[0003] The conventional LTCC substrate co-firing process is to place the LTCC substrate embryo on a support plate. The sintering process is free of any constraints and the substrate shrinks freely. Due to the problem of asynchronous sintering shrinkage of the conductor slurry and the green porcelain, the first warping often occurs during the sintering process due to the first shrinking substance, and then the second shrinking substance flattens the first warping during the final shrinkage. This process is extremely complicated, so free sintering has strict requirements on the arrangement of the conductor slurry in the substrate, limiting the flexibility of circuit design or process design. Even so, warping of co-fired substrates is still a problem in the industry.
[0004] Based on the continuous pursuit of high-flatness sintering, the industry has also conducted relevant research on constrained sintering. The patents "Flexible porous metal foil and its preparation method" and "Diaphragm sintering tooling" both disclose a tooling for constrained sintering of diaphragms, but the tooling clamping plate needs to be in pressure contact with the diaphragm, which will affect the sintering shrinkage rate in the XY direction and cannot be used for LTCC substrates that have high requirements for sintering shrinkage accuracy. The patents "Constrained sintering method of asymmetric dielectrics" and "Constrained sintering method of low-temperature co-fired ceramic structures with pseudo-symmetric structures" both disclose a method of stacking self-constrained tapes and primary tapes, using the difference in glass rigidity temperature between different raw ceramic tapes to achieve mutual suppression of the overall XY sintering shrinkage of the substrate, thereby achieving the purpose of improving the flatness of the substrate. However, this structure requires the substrate to contain raw ceramic tapes with different properties, and has extremely complex requirements for raw ceramic materials and circuit design, and cannot be applied to common commercial LTCC materials.
[0005] The paper "Research on the Flatness of LTCC Substrate Co-firing" improves the flatness of LTCC substrate co-firing through layout optimization; the paper "Research on Low-Temperature Co-fired Ceramic (LTCC) Process" mentions the conventional LTCC co-firing process; the paper "Research on Matching Co-firing of LTCC Heterogeneous Materials" improves the matching of heterogeneous materials co-firing from the formula; the paper "Research Progress on Preparation Technology of Low-Temperature Co-firing Ceramic Substrates" reviews the sintering reaction mechanism of LTCC substrates; the paper "Research on the Low-Temperature Co-firing of Silver-based Multilayer Aluminum Nitride Ceramic Substrates" realizes the silver wiring of multilayer aluminum nitride through the secondary debinding method and the method of adding trace oxygen to the nitrogen atmosphere for sintering. However, these studies are all in-depth discussions on the co-firing process itself, and do not involve constrained sintering for the purpose of improving the flatness of the substrate.
[0006] In view of the urgent need for high co-firing flatness of LTCC substrates, it is urgent to develop a new co-firing process that is compatible with most commercial LTCC materials to improve the final sintering flatness of LTCC substrates. Summary of the invention
[0007] In order to solve the above problems, the present invention proposes a pressureless constrained sintering method for LTCC substrates, which is compatible with most commercial LTCC materials and can reduce the warping of the substrate during the sintering process and improve the flatness of the final LTCC substrate without changing the circuit design, process design, and sintering conditions.
[0008] The technical solution adopted by the present invention is as follows:
[0009] A pressureless constrained sintering method for a LTCC substrate, comprising:
[0010] When green ceramic lamination is performed based on LTCC (low temperature co-fired ceramic) technology, a forced pressing sheet is arranged on the upper surface of the green ceramic body to forcefully press the raised part to obtain a LTCC body with a smooth surface;
[0011] The LTCC embryo, the follower support block and the restraining plate are placed on the setter plate according to relative positions; a plurality of the follower support blocks are provided and are evenly arranged around the LTCC embryo; the restraining plate is arranged directly above the LTCC embryo and is supported by the follower support block and does not contact the LTCC embryo;
[0012] Based on the LTCC co-firing equipment and sintering conditions, the LTCC embryonic body with the follower support block and the constraint pressing plate is sintered to achieve the firing of the LTCC ceramic substrate with high flatness.
[0013] Furthermore, the method of setting a forced pressing sheet on the upper surface of the green porcelain body to force pressure on the raised portion includes: adding a copper sheet or a stainless steel sheet of preset thickness on the upper surface of the green porcelain body as a forced pressing sheet, and by force pressurizing the raised portion, eliminating the undulations on the substrate surface caused by the internal wiring arrangement, thereby obtaining a flat surface, and the thickness deviation of each position of the LTCC body after lamination should be less than a first preset value.
[0014] Furthermore, the thickness of the forced tableting ranges from 0.1 mm to 0.3 mm.
[0015] Furthermore, the first preset value of the thickness deviation of each position of the LTCC embryo body includes: 0.03 mm.
[0016] Furthermore, the follower support block can be flexibly placed around the LTCC embryo, the support constraint plate does not contact the LTCC embryo in the initial sintering stage, and the distance between the lower surface of the constraint plate and the upper surface of the LTCC embryo is at a second preset value, and the thickness of the follower support block decreases synchronously with the LTCC embryo during the sintering process.
[0017] Furthermore, the value range of the second preset value includes: 0.03-0.08 mm.
[0018] Furthermore, the difference between the thickness of the follower support block and the thickness of the LTCC embryo body is a third preset value, and the value range of the third preset value includes: 0.05mm~0.1mm.
[0019] Furthermore, the material of the follower support block includes a green ceramic tape that is the same as that of the LTCC embryo.
[0020] Furthermore, the material of the restraining plate includes a high temperature resistant ceramic sheet, and the high temperature resistant ceramic sheet includes an alumina ceramic sheet or a quartz sheet.
[0021] Furthermore, the thickness of the constraining pressing plate shown is in the range of 1 mm to 2 mm, the surface flatness is ≤0.01 mm, the surface roughness is ≤0.003 mm, and it does not adhere to the LTCC dielectric material and the conductor paste at high temperatures.
[0022] The beneficial effects of the present invention are:
[0023] The pressureless constrained sintering method proposed in the present invention can effectively improve the flatness of the LTCC substrate after the final sintering shrinkage by setting a non-contact constrained platen in the initial state and a support block with a thickness that changes dynamically, and accurately controlling the initial distance from the surface of the constrained platen to the surface of the LTCC embryo, thereby suppressing the shrinkage and warping of the embryo, and can effectively improve the flatness of the LTCC substrate after the final sintering shrinkage. Without changing the circuit design, process design, and sintering conditions, the present invention can reduce the warping of the substrate during the sintering process and improve the flatness of the final LTCC substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Schematic diagram of making a highly flat substrate embryo.
[0025] Figure 2 Schematic diagram of stacking products and restraining platens.
[0026] Figure 3 Schematic diagram of deformation and warping during sintering process.
[0027] Figure 4 Schematic diagram of final sintering.
[0028] Figure numerals: 1 is the LTCC embryo, 2 is the laminated backplane, 3 is the forced pressing plate, 4 is the sintering plate, 5 is the restraining pressing plate, and S is the follower support block; 1-A is the substrate embryo during the sintering process, 1-C is the LTCC substrate after the final sintering; S-1 is the follower support block during the sintering process, and S-2 is the follower support block after the final sintering. DETAILED DESCRIPTION
[0029] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present invention.
[0030] Example 1
[0031] like Figure 1 As shown, this embodiment provides a pressureless constrained sintering method for a LTCC substrate, comprising:
[0032] When green ceramic lamination is performed based on LTCC (low temperature co-fired ceramic) technology, a forced pressing sheet is arranged on the upper surface of the green ceramic body to forcefully press the raised part to obtain a LTCC body with a smooth surface;
[0033] The LTCC embryo, the follower support block and the restraining plate are placed on the setter plate according to relative positions; a plurality of the follower support blocks are provided and are evenly arranged around the LTCC embryo; the restraining plate is arranged directly above the LTCC embryo and is supported by the follower support block and does not contact the LTCC embryo;
[0034] Based on the LTCC co-firing equipment and sintering conditions, the LTCC embryonic body with the follower support block and the constraint pressing plate is sintered to achieve the firing of the LTCC ceramic substrate with high flatness.
[0035] Specifically, the pressureless constrained sintering method of this embodiment mainly includes the steps of making a high-flatness substrate embryo, setting a follower support block, selecting a constrained pressing plate, product stacking, and co-firing.
[0036] Among them, the production of high-flatness substrate embryos is that when laminating the LTCC green porcelain, a copper sheet or a stainless steel sheet of preset thickness (for example, 0.1mm-0.3mm) is added to the upper surface of the green porcelain embryo as a forced pressing sheet, and the undulations on the substrate surface caused by the internal wiring arrangement are eliminated by forced pressure on the raised parts to obtain a flat surface. After lamination, the thickness deviation of each position of the LTCC embryo should be ≤ a first preset value (for example, 0.03mm).
[0037] Preferably, the follower support block can be flexibly placed around the LTCC embryo, the support and restraining plate does not contact the LTCC embryo in the initial stage of sintering, and the distance between the lower surface of the restraining plate and the upper surface of the LTCC embryo is at a second preset value (for example, 0.03 to 0.08 mm), and its thickness decreases synchronously with the LTCC embryo during the sintering process.
[0038] Preferably, the follower support block is made of a green ceramic tape that is the same as the LTCC embryo body, and its thickness is greater than the thickness of the LTCC embryo body by a third preset value (eg, 0.05 mm to 0.1 mm).
[0039] Preferably, the material of the restraining plate is usually a high temperature resistant ceramic sheet such as 96 alumina ceramic sheet, 99 alumina ceramic sheet, quartz sheet, etc., with a thickness of generally 1mm to 2mm, a surface flatness of ≤0.01mm, a surface roughness of ≤0.003mm, and no adhesion to the LTCC dielectric material and conductor paste at high temperature.
[0040] Preferably, the product is stacked by placing the LTCC embryo, the follower support block, and the restraining plate on the firing plate according to relative positions, the follower support blocks are evenly placed around the LTCC embryo, the number is ≥4, the restraining plate is placed directly above the LTCC embryo, and is supported by the follower support blocks without contacting the LTCC embryo.
[0041] Preferably, the co-firing is to utilize conventional LTCC co-firing equipment and sintering conditions to sinter the LTCC embryonic body with the follower support block and the restraining plate stacked, thereby finally achieving the firing of a highly flat LTCC ceramic substrate.
[0042] Example 2
[0043] This embodiment is based on embodiment 1:
[0044] This embodiment provides a pressureless constrained sintering method for a LTCC substrate, comprising the following steps:
[0045] like Figure 1As shown, JC29 raw porcelain with a thickness of 0.127 mm produced by China Building Materials Academy was selected, and the silver paste for hole filling Ag01, the silver paste for inner wiring Ag02, and the silver paste for surface wiring Ag12 were matched to make a 10-layer LTCC circuit substrate with a plane size of 50 mm × 50 mm. The laminated raw porcelain body was placed on the laminated backplane 2, and a 0.3 mm thick forced pressing sheet 3 was placed on the surface of the raw porcelain body. The other conventional LTCC lamination process conditions were adopted, with a lamination pressure of 3200 PSI and a lamination temperature of 70°C. The total thickness of the LTCC body 1 after lamination was 1.22 mm to 1.23 mm.
[0046] like Figure 2 As shown, the laminated LTCC embryonic body 1 is placed on a conventional setter plate 4 .
[0047] like Figure 2 As shown, the follower support block S is made of JC29 type raw porcelain, with a total thickness of 1.28 mm and a plane size of 10 mm×10 mm.
[0048] like Figure 3 As shown, during the sintering process, the LTCC embryo 1 will warp, that is, the substrate embryo 1-A, which is constrained by the constraint plate 5 so that the substrate embryo 1-A will not warp too much. The follower support block S is transformed into the follower support block S-1, and the thickness of the follower support block S-1 changes synchronously with the substrate embryo 1-A.
[0049] like Figure 4 As shown, during the process of the LTCC embryo 1 shrinking and densifying to the ceramic body, namely the LTCC substrate 1-C, the follower support block S shrinks and densifies to the follower support block S-2, whose thickness is still higher than that of the LTCC substrate 1-C. While restraining the excessive warping of the LTCC substrate 1-C, it does not affect the free shrinkage of the LTCC substrate 1-C, thereby taking into account both high flatness and high shrinkage rate accuracy.
[0050] It should be noted that, for the aforementioned method embodiments, for the sake of simplicity of description, they are expressed as a series of action combinations, but those skilled in the art should be aware that the present application is not limited by the order of the actions described, because according to the present application, certain steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also be aware that the embodiments described in the specification are all preferred embodiments, and the actions and modules involved are not necessarily required by the present application.
Claims
1. A pressureless constrained sintering method for a LTCC substrate, characterized in that: include: When green ceramic lamination is performed based on LTCC (low temperature co-fired ceramic) technology, a forced pressing sheet is arranged on the upper surface of the green ceramic body to forcefully press the raised part to obtain a LTCC body with a smooth surface; The LTCC embryo, the follower support block and the restraining plate are placed on the setter plate according to relative positions; a plurality of the follower support blocks are provided and are evenly arranged around the LTCC embryo; the restraining plate is arranged directly above the LTCC embryo and is supported by the follower support block and does not contact the LTCC embryo; Based on the LTCC co-firing equipment and sintering conditions, the LTCC embryonic body with the follower support block and the constraint pressing plate is sintered to achieve the firing of the LTCC ceramic substrate with high flatness.
2. A pressureless constrained sintering method for a LTCC substrate according to claim 1, characterized in that: The method of setting a forced pressing sheet on the upper surface of the raw porcelain body to force pressure on the raised part includes: adding a copper sheet or a stainless steel sheet of preset thickness on the upper surface of the raw porcelain body as a forced pressing sheet, and by force pressurizing the raised part, eliminating the undulations on the surface of the substrate caused by the internal wiring arrangement, obtaining a flat surface, and after lamination, the thickness deviation of each position of the LTCC body should be less than a first preset value.
3. The pressureless constrained sintering method of a LTCC substrate according to claim 2, characterized in that: The thickness of the forced tableting ranges from 0.1 mm to 0.3 mm.
4. The method for pressureless constrained sintering of a LTCC substrate according to claim 2, characterized in that: The first preset value of the thickness deviation of each position of the LTCC embryo body includes: 0.03 mm.
5. The method for pressureless constrained sintering of a LTCC substrate according to claim 1, characterized in that: The follower support block can be flexibly placed around the LTCC embryo, the support constraint plate does not contact the LTCC embryo in the initial sintering stage, and the distance between the lower surface of the constraint plate and the upper surface of the LTCC embryo is at a second preset value, and the thickness of the follower support block decreases synchronously with the LTCC embryo during the sintering process.
6. The method for pressureless constrained sintering of a LTCC substrate according to claim 5, characterized in that: The value range of the second preset value includes: 0.03-0.08 mm.
7. The method for pressureless constrained sintering of a LTCC substrate according to claim 5, characterized in that: The difference between the thickness of the follower support block and the thickness of the LTCC embryo body is a third preset value, and the value range of the third preset value includes: 0.05mm~0.1mm.
8. The method for pressureless constrained sintering of a LTCC substrate according to claim 1, characterized in that: The material of the follower support block includes the same green ceramic tape as the LTCC embryo body.
9. The method for pressureless constrained sintering of a LTCC substrate according to claim 1, characterized in that: The material of the restraining plate shown includes a high temperature resistant ceramic sheet, and the high temperature resistant ceramic sheet includes an alumina ceramic sheet or a quartz sheet.
10. The method for pressureless constrained sintering of a LTCC substrate according to claim 1, characterized in that: The thickness of the restraining plate shown in the figure ranges from 1 mm to 2 mm, the surface flatness is ≤0.01 mm, the surface roughness is ≤0.003 mm, and it does not adhere to the LTCC dielectric material and the conductor paste during the high-temperature sintering process.
Citation Information
Patent Citations
Control technological method for planeness of surface of LTCC substrate
CN102724822A
High-temperature pressure sensor and production method thereof
CN103115704A
Sintering method for large-sized high-temperature co-fired ceramics
CN109053196A
Manufacturing method of LTCC substrate with two-sided cavity structure
CN109309060A
Flake ceramic pressing sintering device and using method thereof
CN113916002A