Preparation method of low-temperature fast curing polyurethane film material
Through the reaction system of cyanate, polyol and catalyst, the molar ratio and heating conditions are adjusted, the problem of long curing time of polyurethane film materials is solved, and the low-temperature rapid curing and high-performance polyurethane film materials are achieved, which are suitable for many industrial fields.
Patent Information
- Application Number
- CN202411226516.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-09-03
AI Technical Summary
The domestically prepared polyurethane film materials have a long curing time and have not met the requirements of rapid curing, which limits their wide application in automobile manufacturing, construction and other fields.
Using a reaction system of cyanate ester, polyol, chain extender and catalyst, a low-temperature rapid curing polyurethane film material was developed by adjusting the molar ratio and heating conditions, achieving low heat exothermic value and rapid molding.
The prepared materials have low viscosity, rapid curing, good film forming performance and low small molecule content. They are suitable for automobile manufacturing, construction engineering, aerospace and electronic products, and improve the mechanical properties and self-repair properties of the materials.
Smart Images

Figure CN118894977A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of organic polymer material preparation, and in particular relates to a method for preparing a low-temperature fast-curing polyurethane film material. Background Art
[0002] Polyurethane is composed of hard segments and soft segments. The hard segment is mainly composed of isocyanate and small molecule chain extender, and its proportion will affect the heat resistance, mechanical properties, hardness, etc. of polyurethane materials. The soft segment is composed of diols or diamines, and its relative molecular mass is higher than that of isocyanate and small molecule chain extender. Its proportion will affect the elasticity, crystallization, flexibility, etc. of polyurethane. The crystallization produced by hydrogen bonds in the hard segment and the soft segment will cause microphase separation between the soft segment and the hard segment. There is an island structure inside the polyurethane material, which has the functions of reinforcement and physical cross-linking, giving the polyurethane material excellent performance. With its good elasticity and impact resistance, excellent waterproof performance, wear and corrosion resistance, and high chemical stability, polyurethane has broad development prospects in the fields of automobile manufacturing, construction, and medical equipment.
[0003] At present, most of the polyurethane film materials prepared in China have a long curing time, averaging about several hours, which is far from meeting the requirements of rapid curing. The purpose of the present invention is to prepare a low-temperature rapid curing polyurethane film material to achieve the domestic preparation and application of low-cost materials. Summary of the invention
[0004] In view of this, the present invention proposes a method for preparing a low-temperature rapid curing polyurethane film material, which is prepared by a reaction system consisting of cyanate ester, polyol, chain extender and catalyst, and is used for rapid curing into a high-gloss surface, and should have the characteristics of low exothermic value and fast molding speed. The in-mold painted polyurethane material developed by this method not only has the advantages of low viscosity, rapid curing, good film-forming performance, and low small molecule content, but can also be used in the fields of construction engineering, automobile manufacturing, aerospace, and electronic products.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] A method for preparing a low-temperature fast-curing polyurethane film material comprises the following steps:
[0007] A1: 1 mol of 1,4-butanediol and dehydrated polytetrahydrofuran were added and mixed, and then 5 g of DMF was added and mixed, and then 2 mol of diphenylmethane diisocyanate, 0.2 g of dibutyltin dilaurate and 15 g of DMF were added and heated to react to form a prepolymer;
[0008] A2: Increase the molar ratio of diphenylmethane diisocyanate, polytetrahydrofuran and 1,4-butanediol to 2-3:1:1 to increase the R value (-NCO / -OH) to 1.3, because the -NCO group in the isocyanate will react with the moisture in the air to form a urea group, thereby losing a part of the -NCO group. Add the remaining diphenylmethane diisocyanate three times, stir, and add 4g DMF each time; after the reaction is complete, evacuate the mixture under vacuum, pour the treated mixture on a glass plate to coat it into a film, and heat and cure to obtain the low-temperature fast-curing polyurethane film material.
[0009] Preferably, in step A1, the dehydration temperature of polytetrahydrofuran is 110° C., and the dehydration time is 2 h; the speed of the stirrer is 200-300 r / min, preferably 300 r / min;
[0010] The heating reaction temperature is 70-80°C, preferably 70°C; the heating reaction time is 2h.
[0011] Preferably, in step A2, the molar ratio of diphenylmethane diisocyanate, polytetrahydrofuran and 1,4-butanediol is preferably 2.6:1:1.
[0012] Preferably, the operation of adding the remaining diphenylmethane diisocyanate in three times is as follows:
[0013] The first stirring was 30 min, the second stirring was 1 h, and the third stirring was 30 min.
[0014] Preferably, in step A2, the curing temperature is 80-90° C., preferably 90° C.; and the coating thickness is 500 μm.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] The present invention uses polytetramethylene glycol (PTMEG) as a diol, diphenylmethane diisocyanate (MDI) as an isocyanate, 1,4-butanediol (BDO) as a chain extender, and dibutyltin dilaurate as a catalyst to react and prepare a low-temperature fast-curing polyurethane membrane material. The composed material system is simple, efficient and low-cost, which is conducive to industrial production. The low-temperature fast-curing polyurethane membrane material obtained by the preparation method can be used in the fields of automobile manufacturing, construction engineering, aerospace, and electronic products.
[0017] The present invention introduces PTMEG diol to react with MDI under the catalyst DBTDL, so that the polyurethane coating is quickly cured and formed within 2 minutes at 90° C., and introduces the chain extender BDO to form more hydrogen bonds between the molecular chains. The high-density hydrogen bonding effect enables the material to have higher mechanical properties and self-healing properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0019] Figure 1 This is a schematic diagram of the preparation of a fast-curing polyurethane film according to the present invention.
[0020] Figure 2 Schematic diagram of infrared spectrum of 1000 molecular weight PTMEG-based MDI polyurethane film.
[0021] Figure 3 Schematic diagram of infrared spectrum of 2000 molecular weight PTMEG-based MDI polyurethane film.
[0022] Figure 4 Schematic diagram of infrared spectrum of p-phenylene diisocyanate (PPDI) type polyurethane film.
[0023] Figure 5 Schematic diagram of the infrared spectrum of isophorone diisocyanate (IPDI) type polyurethane film. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this application are performed using conventional test methods in the art. It should be understood that the terms described in this application are only used to describe specific implementation methods and are not used to limit the content disclosed in this application.
[0026] Unless otherwise specified, the technical and scientific terms used in this document have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs; other experimental methods and technical means not specifically specified in this application refer to experimental methods and technical means commonly used by ordinary technicians in this field.
[0027] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present application.
[0028] Under the premise of no conflict, the technical features disclosed in the embodiments of the present application can be combined arbitrarily, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present application.
[0029] The invention discloses a method for preparing a low-temperature fast-curing polyurethane film material.
[0030] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as a limitation of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.
[0031] Embodiment 1:
[0032] In this embodiment, polytetrahydrofuran is used as the diol, diphenylmethane diisocyanate is used as the isocyanate, dibutyltin dilaurate is used as the catalyst, and 1,4-butanediol is used as the chain extender. After the diol and isocyanate are prepolymerized successfully, an appropriate amount of isocyanate is added to increase the molar ratio to 2.6:1:1, and finally a coating and low-temperature curing are performed to prepare a fast-curing polyurethane film material. The preparation flow chart is shown in FIG. Figure 1 As shown, the specific method is as follows:
[0033] (1) Add 1 mol each of polytetrahydrofuran and 1,4-butanediol and 5 g of DMF into a flask and stir for 30 min.
[0034] (2) 2 mol of MDI, 0.2 g of DBTDL and 15 g of DMF were added into a flask and heated and stirred at 70°C and 300 r / min for 2 h to form a prepolymer.
[0035] (3) After the prepolymerization, the molar ratio of diphenylmethane diisocyanate, polytetrahydrofuran and 1,4-butanediol was increased to 2.6:1:1, and the remaining 0.6 mol of MDI was added to the prepolymer in three times. The first time, 0.39 g was added and stirred for reaction for 30 min. The second time, 0.48 g was added and stirred for reaction for 1 h. The third time, 0.31 g was added and stirred for reaction for 30 min. 4 g of DMF was added each time to reduce its viscosity.
[0036] (4) After all reactions are completed, the synthesized polyurethane adhesive is placed in a vacuum oven at 60°C to remove bubbles for 30 minutes.
[0037] (5) Spray a layer of release agent on the glass plate and heat it in an oven for 5 minutes. Finally, use a 500 μm coating rod to evenly coat the polyurethane glue on the glass plate. Place the glass plate in an oven at 90 °C to heat and cure it into a film, and record the curing time.
[0038] (6) After heating, the polyurethane film is desorbed from the glass plate to obtain a fast-curing polyurethane film.
[0039] Embodiment 2:
[0040] In this embodiment, polytetrahydrofuran is used as the diol, diphenylmethane diisocyanate is used as the isocyanate, dibutyltin dilaurate is used as the catalyst, and 1,4-butanediol is used as the chain extender. After the diol and the isocyanate are prepolymerized successfully, an appropriate amount of isocyanate is added to increase the molar ratio to 3:1:1, and finally the film is coated and low-temperature cured to prepare the polyurethane film material. The specific method is as follows:
[0041] (1) Add 1 mol each of polytetrahydrofuran and 1,4-butanediol and 5 g of DMF into a flask and stir for 30 min.
[0042] (2) 2 mol of MDI, 0.2 g of DBTDL and 15 g of DMF were added into a flask and heated and stirred at 70°C and 300 r / min for 2 h to form a prepolymer.
[0043] (3) After the prepolymerization, the molar ratio of diphenylmethane diisocyanate, polytetrahydrofuran and 1,4-butanediol was increased to 3:1:1, and the remaining 1 mol of MDI was added to the prepolymer in three times. The first time, 0.40 g was added and stirred for reaction for 30 min. The second time, 0.72 g was added and stirred for reaction for 1 h. The third time, 0.31 g was added and stirred for reaction for 30 min. 4 g of DMF was added each time.
[0044] (4) After all reactions are completed, the synthesized polyurethane adhesive is placed in a vacuum oven at 60°C to remove bubbles for 30 minutes.
[0045] (5) Spray a layer of release agent on the glass plate and heat it in an oven for 5 minutes. Finally, use a 500 μm coating rod to evenly coat the polyurethane glue on the glass plate. Place the glass plate in an oven at 90 °C to heat and cure it into a film, and record the curing time.
[0046] (6) After heating, the polyurethane film is desorbed from the glass plate to obtain a fast-curing polyurethane film.
[0047] In order to further demonstrate the beneficial effects of the present invention and to better understand the present invention, the following test examples are used to further illustrate the technical features disclosed in the present invention, but they should not be understood as limiting the present invention. Other improvements made by those skilled in the art based on the above invention content without creative work are also considered to fall within the scope of protection of the present invention.
[0048] Test example:
[0049] (1) The infrared spectrum diagram of the 1000 molecular weight PTMEG-based MDI polyurethane film of this example is shown in Figure 2 As shown, from Figure 2 As can be seen in (a) and (b), the characteristic peaks of PTMEG include CH at 2934 cm -1 and 2850cm -1 The bending vibration absorption peak of -CH2- is at 1447cm -1 and 1367cm -1 、-OH at 1235 cm -1 The in-plane bending vibration absorption peak at 1100 cm -1 The characteristic peak of MDI is mainly -NCO at 2255 cm -1 In the infrared spectrum of PU, a C=O stretching vibration absorption peak is located at 1591 cm -1 -1741cm -1 and an ether bond stretching vibration absorption peak at 1104 cm -1 The asymmetric stretching vibration absorption peak of -NCO is at 2253 cm -1 As the reaction proceeds, the FTIR absorption intensity of -NCO gradually decreases (Figure b), which indicates that the reaction of MDI and PTMEG is successful, and the isocyanate group reacts with the hydroxyl group to form carbamate, producing the expected product.
[0050] The curing time of the polyurethane film cured at 90°C is 7 minutes. The film is transparent as a whole, has good elasticity and high adhesion.
[0051] (2) The infrared spectrum diagram of the 2000 molecular weight PTMEG-based MDI polyurethane film of this example is shown in FIG. Figure 3 As shown, from Figure 3 It can be seen that the -NCO characteristic peak in the infrared spectrum of the PU film is at 2253 cm -1 has disappeared, indicating that MDI has reacted completely, -NCO reacts with -OH to form carbamate, and the expected polyurethane product is produced.
[0052] The curing time of the polyurethane film cured at 90°C is 2 minutes. The synthesized polyurethane glue is yellowish, the film is transparent as a whole, has high adhesion and high elasticity.
[0053] (3) The infrared spectrum diagram of the polyurethane film of PPDI type in this example is as follows: Figure 4 As shown, from Figure 4 It can be seen from the infrared spectrum of PU film that 2220cm -1 ~2280cm -1 The characteristic peaks of -NCO disappeared in the PU samples, indicating that all -NCO groups reacted with -OH groups, and the PPDI type polyurethane film was successfully synthesized. The curing time of the polyurethane film cured at 90℃ was 3min, and the film was matte in color.
[0054] (4) The infrared spectrum diagram of the isophorone diisocyanate (IPDI) type polyurethane film in this example is shown in FIG. Figure 5 As shown, from Figure 5 It can be seen that the polyurethane films synthesized by PTMEG, IPDI and BDO have a wavelength of 2270 cm -1 There is no characteristic peak nearby, that is, the -NCO group has reacted completely and there is no free -NCO group in the system, indicating that the IPDI type polyurethane film was successfully prepared. The curing time of the polyurethane film cured at 90°C is 7min, the film is transparent as a whole, the mechanical properties are poor, and the adhesion is high.
[0055] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a low-temperature rapid curing polyurethane film material, characterized in that: The steps include: A1: 1 mol of 1,4-butanediol and dehydrated polytetrahydrofuran were added and mixed, and then 5 g of DMF was added and mixed, and then 2 mol of diphenylmethane diisocyanate, 0.2 g of dibutyltin dilaurate and 15 g of DMF were added and heated to react to form a prepolymer; A2: The molar ratio of diphenylmethane diisocyanate, polytetrahydrofuran and 1,4-butanediol is increased to 2-3:1:1, and the remaining diphenylmethane diisocyanate is added three times with stirring, and 4 g of DMF is added each time; after the reaction is complete, the mixture is evacuated under vacuum, and the treated mixture is poured on a glass plate to form a film, and heated and cured to obtain the low-temperature fast-curing polyurethane film material.
2. The method for preparing a low-temperature rapid curing polyurethane film material according to claim 1, characterized in that: In step A1, the dehydration temperature of polytetrahydrofuran is 110° C., the dehydration time is 2 h, and the speed of the stirrer is 200-300 r / min; The heating reaction temperature is 70~80℃ and the heating reaction time is 2h.
3. The method for preparing a low-temperature rapid curing polyurethane film material according to claim 1, characterized in that: The operation of adding the remaining diphenylmethane diisocyanate three times is as follows: The first stirring was 30 min, the second stirring was 1 h, and the third stirring was 30 min.
4. The method for preparing a low-temperature rapid curing polyurethane film material according to claim 1, characterized in that: In step A2, the curing temperature is 80-90° C. and the coating thickness is 500 μm.
Citation Information
Patent Citations
Hybrid diisocyanate polyurethane and preparation method hereof
CN106832186A
Polyurethane, preparing method therefor, and use thereof
WO2016159723A1
Cited By
Rapidly-cured polyurethane protective paint as well as preparation method and application thereof
CN119823637A