Preparation method and preparation device of porous foam hydrogel and drug delivery device

By mixing hydrogel precursors with gas, extruding them through a sieve to create bubbles, and then cross-linking and solidifying them, the problems of uneven pore structure and poor connectivity in the preparation of porous foam hydrogels are solved, thus achieving the preparation of porous foam hydrogels with simplified preparation process and improved biocompatibility.

CN118895014APending Publication Date: 2024-11-05ZHENGZHOU UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202311282179.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-09-28
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing technologies struggle to prepare porous foam hydrogels with uniform pore structure and good connectivity, and the preparation process is complex, may contain harmful reagents, and has poor biocompatibility.

Method used

A porous foam hydrogel is formed by mixing a hydrogel precursor with a crosslinking agent and then extruding it through a screen under pressure. The mixture is then crosslinked and cured under the action of the crosslinking agent. The curing is carried out using photo or chemical crosslinking agents without the need for surfactants.

Benefits of technology

A porous foam hydrogel with uniform pore structure and good connectivity was prepared, which has good swelling and adhesion properties and is suitable for biomedical materials such as skin dressings. The preparation process is simplified and it has good biocompatibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895014A_ABST
    Figure CN118895014A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of porous foam hydrogel, which comprises the following steps: mixing a hydrogel precursor with a cross-linking agent to obtain a mixed solution; mixing the mixed solution with gas, foaming through a screen mesh, and crosslinking and curing the obtained foam to obtain porous foam hydrogel; and the aperture of the screen mesh is 100 to 1000 meshes. According to the method provided by the invention, reagents such as a surfactant, a foaming agent and a pore-foaming agent do not need to be added, so that the obtained porous foam hydrogel has a communicated pore structure, is more suitable for being used as biomedical materials such as skin dressings, soft tissue filling and hemostatic materials, is low in toxicity and good in biocompatibility, does not need to be further treated by melting or freeze drying and the like, and is suitable for large-scale production. And the preparation process can be simplified.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of medical devices, and more specifically, to a method for preparing a porous foam hydrogel, a preparation device and a drug delivery device. Background Art

[0002] Foam hydrogel refers to a porous hydrogel with a pore structure. It has excellent biocompatibility, excellent adsorption performance, large specific surface area and adjustable mechanical properties. It can be used as a tissue engineering scaffold, drug carrier, skin dressing, etc.

[0003] Biomaterials that can form foam hydrogels in situ are useful for various applications, especially for materials used as skin dressings. The formation of foam hydrogels directly on the wound part is not only beneficial for drug delivery, but also for the absorption of tissue exudate, air permeability, etc., providing a microenvironment that is conducive to tissue regeneration. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a method for preparing a porous foam hydrogel, a preparation device and a drug delivery device. The porous foam hydrogel provided by the present invention can be formed in situ and has good adhesion and porous structure.

[0005] The present invention provides a method for preparing a porous foam hydrogel, comprising:

[0006] mixing a hydrogel precursor with a cross-linking agent to obtain a mixed solution;

[0007] The mixed solution is mixed with gas and then foamed through a screen, and the obtained foam is cross-linked and solidified to obtain a porous foam hydrogel;

[0008] The aperture of the sieve is 100-1000 meshes.

[0009] The invention first mixes a hydrogel precursor and a crosslinking agent, then mixes with gas and forms foam by screening under extrusion conditions, and crosslinks and solidifies under the action of the crosslinking agent to obtain in situ a porous foam hydrogel with uniform pore structure and good connectivity.

[0010] In the present application, a hydrogel precursor refers to a solution that can form a hydrogel after cross-linking, such as a natural polymer solution, including but not limited to a silk fibroin solution, a gelatin solution, an alginate solution, a hyaluronic acid solution, a collagen solution, a chitosan solution and a functionalized product solution thereof, such as a functionalized silk fibroin solution, a functionalized alginate solution, a functionalized gelatin solution, a functionalized chitosan solution, a functionalized hyaluronic acid solution, and a functionalized collagen solution. In some specific implementations, the functionalized product refers to a natural polymer modified with a cross-linkable group, such as functionalizing it with methacrylic anhydride to obtain a methacrylated natural polymer, such as methacrylate gelatin, which is beneficial for subsequent cross-linking and curing under the action of a cross-linking agent such as a photoinitiator to form a porous foam hydrogel.

[0011] In some specific implementations, the concentration of the hydrogel precursor is 1 wt% to 30 wt%, preferably 5 wt% to 30 wt%, and more preferably 5 wt% to 25 wt%.

[0012] In the present application, the role of the crosslinking agent is to crosslink and cure the hydrogel precursor after forming a foam structure to maintain the foam structure. In some specific implementations, the crosslinking agent is a photoinitiator. At this time, the crosslinking and curing is crosslinking and curing under light conditions. It can be understood in the art that when crosslinking and curing with a photoinitiator, the hydrogel precursor can be functionalized so that it can be crosslinked and cured under the action of the photoinitiator. In some specific implementations, the photoinitiator includes but is not limited to lithium phenyl-2,4,6-trimethylbenzoylphosphonate (LAP), IRGACURE 2959, IRGACURE784, safranineO Safranine-based, eosin Y, Ru(bpy)3 2+ , zinc tetraphenylporphyrin (ZnTPP) or TPO, preferably LAP. The present application has no special restrictions on the parameters of photocuring crosslinking, which can be determined according to the selected photoinitiator.

[0013] In some specific implementations, the crosslinking agent is a chemical crosslinking agent, that is, it reacts chemically with the hydrogel precursor. At this time, the crosslinking curing is a crosslinking curing by standing at room temperature. In some specific implementations, the crosslinking agent includes but is not limited to a mixture of 4-morpholineethanesulfonic acid, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide, glutaraldehyde, epoxy compounds or carbodiimide, etc. In some specific implementations, the ratio of 4-morpholineethanesulfonic acid, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide is 0.001~0.1g: 0.3~0.8mol: 0.1~0.3mol. The present invention has no special restrictions on the parameters of the chemical curing crosslinking, which can be determined according to the selected chemical crosslinking agent.

[0014] In some specific implementations, the cross-linking curing time is 5s to 20min, preferably 30s to 15min, more preferably 1min to 10min. In some specific implementations, the amount of the cross-linking agent is 0.1wt% to 10wt% of the hydrogel precursor, preferably 0.2wt% to 8wt%, more preferably 0.3wt% to 7wt%.

[0015] The present invention first mixes a hydrogel precursor and a crosslinking agent to obtain a mixed solution. As mentioned above, the hydrogel precursor is a solution, and silk fibroin, alginic acid, gelatin, chitosan, hyaluronic acid, collagen and functionalized products thereof are dissolved in a solvent according to a method known to those skilled in the art. The hydrogel precursor and the crosslinking agent are uniformly mixed to obtain a mixed solution.

[0016] After the mixed solution is obtained, it is mixed with gas, and foamed through a screen under extrusion conditions to form foam, and then cross-linked and cured to obtain a porous foam hydrogel. In some specific implementations, the gas includes but is not limited to air, oxygen, argon, nitrogen, etc., preferably air. In some specific implementations, the volume ratio of the gas to the mixed solution is 5:6 to 5:10, preferably 5:7 to 5:9.

[0017] After obtaining the gas-liquid mixture, it is squeezed so that the mixture is squeezed through a screen to form a foam. In some specific implementations, the mesh has an aperture of 100 to 1000 mesh, preferably 150 to 800 mesh, and more preferably 300 to 500 mesh. After the foam is formed, it is cross-linked and cured to form a porous foam hydrogel.

[0018] The present invention also provides a device for preparing a porous foam hydrogel, comprising:

[0019] A hydrogel precursor storage unit storing a hydrogel precursor;

[0020] a cross-linking agent storage unit for storing the cross-linking agent;

[0021] a bubbling unit whose inlet is connected to the hydrogel precursor storage unit and the crosslinking agent storage unit, the bubbling device comprising a gas-liquid mixing chamber, a screen connected to the gas-liquid mixing chamber, and a gas-liquid extrusion device for compressing the gas-liquid mixing chamber;

[0022] A foam receiving unit is connected to the foam outlet of the foaming unit.

[0023] The porous foam hydrogel preparation device provided by the present invention comprises a hydrogel precursor storage unit for storing the hydrogel precursor and a crosslinking agent storage unit for storing the crosslinking agent.

[0024] The preparation device includes a foaming unit, which includes a gas-liquid mixing chamber, a screen connected to the gas-liquid mixing chamber, and an extrusion device for compressing the gas-liquid mixing chamber. Further, the gas-liquid mixing chamber is respectively connected to the hydrogel precursor storage unit and the cross-linking agent storage unit, and the gas-liquid mixing chamber is also provided with a gas inlet for mixing gas and liquid, and then forming foam through the screen under the action of the extrusion device.

[0025] The device provided by the present invention can directly squeeze the foam onto the skin or the required part and solidify it in situ. In some specific implementations, when the crosslinking agent is a chemical crosslinking agent, it can be cured by standing still; in some specific implementations, when the crosslinking agent is a photocrosslinking agent, the device also includes a light unit for light-curing the foam squeezed out by the bubble unit.

[0026] The method provided by the present invention forms foam in situ by means of a gas-liquid mixture being squeezed through a screen to form foam, and in situ crosslinking and curing to obtain a porous foam hydrogel with uniform pore structure, good connectivity and stability. The porous foam hydrogel has good swelling properties, adhesion properties and mechanical properties, and has good effects as a dressing, hemostatic gel or direct or loaded drug application. The method provided by the present application does not require the addition of surfactants, foaming agents, porogens and other reagents, which not only makes the obtained porous foam hydrogel more suitable for use as biomedical materials such as skin dressings, soft tissue fillings, and hemostatic materials, but also has low toxicity and good biocompatibility, and does not require further melting or freeze drying and other treatments, which can simplify the preparation process. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a schematic diagram of the structure of the device for preparing the porous foam hydrogel provided in Example 1 of the present application;

[0028] Figure 2 A schematic structural diagram of a device for preparing a porous hydrogel provided in another embodiment of the present application;

[0029] Figure 3 A foaming device provided for the comparative example of this application.

[0030] Figure 4 This is a scanning electron microscope photograph of the hydrogel prepared in Example 2;

[0031] Figure 5 The scanning electron microscope pictures of the hydrogels prepared in Examples 3 to 5 are shown;

[0032] Figure 6 This is a scanning electron microscope photo of the materials prepared in Comparative Examples 7 to 8;

[0033] Figure 7 The scanning electron microscope photos of the materials prepared in Comparative Example 9 and Example 2 are shown;

[0034] Figure 8 The swelling rate test results of the porous foam hydrogels prepared in Examples 3 to 5;

[0035] Fig. 9 The swelling rate test results of the porous foam hydrogels prepared in Examples 2 and 6 to 8;

[0036] Fig.10 The swelling rate test results of the porous foam hydrogels prepared in Examples 2 and 9 to 12;

[0037] Fig.11 The swelling rate test results of the unfoamed hydrogels prepared in Comparative Examples 1 to 6;

[0038] Fig.12 Compression curves of the porous foam hydrogels prepared in Examples 3 to 5;

[0039] Fig.13 is the compression modulus of the porous foam hydrogel prepared in Examples 3 to 5;

[0040] Fig.14 Compression curves and compression moduli of the hydrogels prepared in Example 2 and Comparative Example 9;

[0041] Fig.15 It is the performance test result of the pigskin of Example 2;

[0042] Fig.16 This is the performance test result of the pigskin of Comparative Example 5;

[0043] Fig.17 This is the performance test result of the pigskin of Comparative Example 9;

[0044] Fig.18 is a lap shear stress-strain diagram of the porous foam hydrogel prepared in Example 4;

[0045] Fig.19 is the lap shear stress-strain diagram of the hydrogel prepared in Comparative Example 5;

[0046] Fig. 20 Pigskin-glass lap test results provided for Example 2 and Comparative Example 9;

[0047] Fig.21 Pigskin-pigskin lap test results provided for Example 2 and Comparative Example 9;

[0048] Fig. 22 is a scanning electron microscope photograph of the porous foam hydrogel prepared in Example 13 of the present application;

[0049] Fig.23 This is a scanning electron microscope photograph of the porous foam hydrogel prepared in Example 14 of the present invention. DETAILED DESCRIPTION

[0050] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0051] Example 1

[0052] See also Figure 1 , Figure 1 This is a schematic structural diagram of a device for preparing a porous foam hydrogel provided in Example 1 of the present application, wherein the device comprises a foaming device and a receiving device.

[0053] The foaming device can be a foaming bottle, which includes a bottle body 1 and a pressing device 2 that can be sealed with the bottle body 1. A screen 21 is provided on the pressing device 2. The mixed liquid of the hydrogel precursor and the cross-linking agent / curing agent in the bottle body 1 is mixed with air under the action of the pressing device 2, passes through the screen to form foam, and is cured in the receiving device 3 to form a porous foam hydrogel.

[0054] In some other embodiments, the preparation device further comprises an illumination device, see Figure 2 , Figure 2 This is a schematic structural diagram of a porous hydrogel preparation device provided in another embodiment of the present application, wherein the preparation device includes a foaming device, a receiving device and an irradiation device 4. At this time, the mixed liquid in the bottle is a hydrogel precursor and a photocuring agent. After the foam is formed through the screen, it is cured by light in the receiving device 3 to form a porous foam hydrogel.

[0055] The illumination device 4 may be an ultraviolet light emitter, a visible light emitter or an infrared light emitter, and is used to emit ultraviolet light, visible light or infrared light to perform light curing on the foam.

[0056] Example 2 Silk fibroin porous hydrogel

[0057] a) boiling the silk cocoons cut into pieces in a 0.02M sodium carbonate solution for 30 minutes for degumming, repeating twice, rinsing with deionized water for three to five times until the sericin is completely rinsed off, and then drying at room temperature;

[0058] b) 20 g of the product obtained in step a) was dissolved in 100 mL of 9.3 M lithium bromide solution at 80° C. for 1 h. After complete dissolution, 6 mL of glycidyl methacrylate (GMA) was slowly added and the reaction was continued for 3 h;

[0059] c) placing the reaction product obtained in step b) into a 3500Da dialysis bag and dialyzing it for 4 days at a dialysis temperature of about 4° C. to prevent the solution from gelling during the dialysis process;

[0060] d) using 100 mL of 50% polyethylene glycol (PEG) to concentrate the dialyzed solution at 4° C. to 15 wt % to obtain a silk fibroin solution;

[0061] e) filtering the silk fibroin solution obtained in step d), and adding 0.5 wt % of a photoinitiator, phenyl-2,4,6-trimethylbenzoylphosphonic acid lithium, to obtain a solution to be foamed;

[0062] f) The solution to be foamed obtained in step e) is foamed by the foaming device provided in Example 1 (the mesh is a plastic or metal stainless steel mesh), and then cross-linked and cured for 10 minutes under the action of ultraviolet rays emitted by an ultraviolet emitter, wherein the mesh number of the mesh in the foaming device is 300 meshes, to obtain a porous foam hydrogel.

[0063] Embodiments 3 to 5

[0064] Compared with Example 2, a 20 wt % silk fibroin solution was used, and the screens in the bubbling device were replaced with 160 mesh, 300 mesh and 500 mesh screens, respectively.

[0065] Embodiments 6 to 8

[0066] Compared with Example 2, the concentrations of the silk fibroin solution in step d) were set to 5wt%, 10wt% and 20wt%, respectively, to obtain porous foam hydrogels.

[0067] Examples 9 to 12

[0068] Compared with Example 2, the cross-linking and curing time in step f) was set to 5 min, 7.5 min, 12.5 min and 15 min, respectively, to obtain porous foam hydrogels.

[0069] Comparative Examples 1 to 6

[0070] Compared with Example 2, the foaming process in step f) was omitted, and cross-linking and curing were directly performed for 1 min, 3 min, 5 min, 7 min, 10 min and 15 min to obtain hydrogels respectively.

[0071] Comparative Example 7

[0072] Compared with Example 2, the solution to be foamed is pumped out with a pipette and irradiated with ultraviolet light for cross-linking and curing to obtain a hydrogel; the obtained hydrogel is placed in deionized water for 24 hours to swell, and freeze-dried after swelling equilibrium is reached. The deionized water in the original hydrogel sublimates and forms pores to obtain a porous foam material.

[0073] Comparative Example 8

[0074] Polylactic acid (PLA) microspheres with consistent pore sizes were dissolved in the foaming solution prepared in Example 2, the obtained solution was pumped out using a pipette, and cross-linked and cured by ultraviolet light to obtain a hydrogel; the obtained hydrogel was placed in dichloromethane, and the PLA microspheres dissolved after 2 hours, and the hydrogel was rinsed with deionized water, swollen for 24 hours, and then freeze-dried to obtain a porous foam hydrogel prepared by a porogen method.

[0075] Comparative Example 9

[0076] See also Figure 3 , Figure 3 The foaming device provided in the comparative example of the present application comprises a three-way pipe 1, two ends of the three-way pipe 1 are respectively connected to a syringe 2 and a syringe 3, and the third end is connected to a needle 4;

[0077] The foaming solution prepared in Example 2 is loaded into syringe 2, and syringe 3 is filled with air. Syringes 2 and 3 are pushed forty times to foam, and then injected into mold 5 through needle end 4, and cross-linked and cured by ultraviolet light to obtain porous foam hydrogel.

[0078] Experimental Example 1

[0079] The materials obtained in Examples 2 to 5 and Comparative Examples 7 to 9 were subjected to electron microscopy scanning. Before the electron microscopy scanning, the obtained hydrogels in Examples 2 to 5 and Comparative Example 9 were pre-frozen at -80°C and then freeze-dried using a freeze dryer to obtain dry materials. The results are shown in Figure 4 , Figure 5 , Figure 6 and Figure 7 , Figure 4This is a scanning electron microscope photo of the hydrogel prepared in Example 2, wherein: Figure 4 (a) is a scanning electron microscope photo of the foam gel obtained by using a plastic mesh screen at a scale of 500 μm. Figure 4 (b) is a scanning electron microscope photograph of the foam gel obtained using a stainless steel mesh screen at a scale of 200 μm; Figure 5 The scanning electron microscope photos of the hydrogels prepared in Examples 3 to 5 are shown in FIG. Figure 5 (a) is a 500 μm scale electron microscope scanning photo of the hydrogel prepared in Example 3. Figure 5 (b) is a scanning electron microscope photograph of the hydrogel prepared in Example 3 at a scale of 200 μm; Figure 5 (c) is a scanning electron microscope photograph of the hydrogel prepared in Example 4, Figure 5 (d) is a scanning electron microscope photograph of the hydrogel prepared in Example 5. Figure 6 This is a scanning electron microscope photo of the material prepared in Comparative Examples 7 to 8, wherein: Figure 6 (a) is a 200 μm scale electron microscope scanning photo of the material prepared in Comparative Example 7, Figure 6 (b) is a 500 μm scale electron microscope scanning photo of the material prepared in Comparative Example 7; Figure 6 (c) is a scanning electron microscope photo of the material prepared in Comparative Example 8 at a scale of 200 μm. Figure 6 (d) is a scanning electron microscope photo of the material prepared in Comparative Example 8 at a scale of 500 μm. Figure 7 The following are scanning electron microscope photos of the materials prepared in Comparative Example 9 and Example 2. Figure 4 and Figure 5 It can be seen that the porous foam hydrogels prepared in Examples 2 to 5 have large and uniform porosity, good connectivity between pores, regular pore size, and smooth pore walls. Among them, the porous foam hydrogel prepared with a 160-mesh screen is a multi-level pore structure of large and small pores, the small pores are approximately 50 to 80 μm, and the large pores are 200 to 500 μm in diameter; the porous foam pores prepared with 300-mesh and 500-mesh screens are relatively uniform, with pore sizes basically between 70 and 210 μm and 70 to 150 μm, and the pores are relatively uniform, and the pore size is consistent with the size that is conducive to cell migration and proliferation.

[0080] Depend on Figure 6 (a) and Figure 6 (b) It can be seen that in the materials prepared by freeze-drying, the pore structure is not connected and the pore wall is generally thick; the surface of the material is a closed pore structure with no connectivity; Figure 6 (c) and Figure 6 (d) It can be seen that in the porous foam hydrogel prepared by the porogen method, the pore size is relatively uniform, but the distribution is uncontrollable, and the pores are closed, which is not conducive to the connectivity of the pores; Figure 7It can be seen that the porous foam prepared in Comparative Example 9 has a very low surface open porosity, and most of the cross-sectional pores are caused by freeze-drying during the freeze-drying process, while the porous foam hydrogel prepared in Example 2 has regular pore size, uniformly connected pores, and smooth pore walls.

[0081] Experimental Example 2

[0082] The porous foam hydrogels prepared in Examples 2 to 12 and Comparative Examples 1 to 6 were tested for swelling rate, and the test method was as follows:

[0083] The prepared porous foam hydrogel was pre-frozen at -80°C and then freeze-dried using a freeze dryer. The freeze-dried hydrogel samples were divided into different components and cut into appropriate sizes for weighing. First, record the dry weight W of each sample. d The dried samples were then immersed in deionized water, and the wet weight W of the samples was measured at 15 min, 30 min, 45 min, 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 24 h, and 48 h. s When measuring the wet weight of the sample, use laboratory wipe paper to slightly absorb excess water on the surface of the hydrogel and then weigh it. Calculate the swelling rate at each time point. The swelling rate W can be expressed as:

[0084] W=(W s -W d )×100% / W d (1);

[0085] Origin software was used for statistical analysis to obtain the swelling rate and swelling equilibrium time of the porous hydrogel.

[0086] Results Figure 8 , Fig. 9 , Fig.10 and Fig.11 , Figure 8 The swelling rate test results of the porous foam hydrogels prepared in Examples 3 to 5 are as follows: Fig. 9 The swelling rate test results of the porous foam hydrogels prepared in Examples 2 and 6 to 8 are as follows: Fig.10 The swelling rate test results of the porous foam hydrogels prepared in Examples 2 and 9 to 12 are as follows: Fig.11 The swelling rate test results of the unfoamed hydrogels prepared in Comparative Examples 1 to 6 are shown in FIG. Figures 8 to 11 It can be seen that the swelling rate of the porous foam hydrogel prepared in Examples 2 to 12 of the present invention can reach more than 3000%, while the swelling rate of the hydrogel obtained without foaming is between 1500% and 2000%.

[0087] Experimental Example 3

[0088] The compression curves and compression moduli of the porous foam hydrogels (wet state) and freeze-dried (dry state) prepared in Examples 2 to 5 and Comparative Example 9 were measured using a universal testing machine. Fig.12 , Fig.13 and Fig.14 , Fig.12 is the compression curve of the porous foam hydrogel prepared in Examples 3 to 5, Fig.13 is the compression modulus of the porous foam hydrogel prepared in Examples 3 to 5, Fig.14 The compression curve and compression modulus of the hydrogel prepared in Example 2 and Comparative Example 9 are shown in FIG. Fig.14 (a) is the compression modulus in wet state, Fig.14 (b) is the compression modulus in dry state. Figure 12 to Figure 14 It can be seen that the porous foam hydrogel obtained in the present application has a higher compression modulus, which is much higher than the compression modulus of the hydrogel prepared in Comparative Example 9.

[0089] Experimental Example 4 Visual Adhesion Test

[0090] The solution to be foamed of Example 2 was extruded onto dry pig skin by the foaming device provided in Example 1 to form foam, and then cross-linked by ultraviolet light for 10 minutes to form a porous foam hydrogel on the pig skin; the solution to be foamed of Comparative Example 5 was directly coated on dry pig skin without foaming, and then cross-linked by ultraviolet light for 10 minutes to form a hydrogel on the pig skin; the solution to be foamed of Comparative Example 9 was injected onto dry pig skin through a needle end after foaming, and cross-linked and cured by ultraviolet light to obtain a porous foam hydrogel.

[0091] The pigskin formed with porous foam hydrogels in Example 2, Comparative Example 5, and Comparative Example 9 were manually subjected to various forces such as stretching, twisting, and bending, and then their wet adhesion was tested by flushing. It was observed whether cracks appeared on the surface of the gel after the force was applied and the water was flushed, and whether the contact part between the gel and the pigskin fell off, to preliminarily test the adhesion and flexibility of the hydrogel. The results are shown in Fig.15 , Fig.16 and Fig.17 ,in, Fig.15 is the performance test result of the pigskin of Example 2, Fig.15 (a) is a pig skin formed into a porous foam hydrogel; Fig.15 (b) is the pigskin after stretching; Fig.15 (c) is the pigskin after twisting; Fig.15 (d) is the pigskin after bending. Fig.15 (e) is pigskin that has been rinsed; Fig.16 This is the performance test result of the pigskin of Comparative Example 5. Fig.16 (a) is the pig skin that directly forms hydrogel without foaming; Fig.16(b) is the pigskin after stretching; Fig.16 (c) is the pigskin after twisting; Fig.16 (d) is the pigskin after bending. Fig.16 (e) is the water treatment of pig skin, Fig.16 (f) is pigskin that has been rinsed; Fig.17 This is the performance test result of the pigskin of Comparative Example 9. Fig.17 (a) is a pig skin formed into a porous foam hydrogel; Fig.17 (b) is the pigskin after stretching; Fig.17 (c) is the pigskin after twisting; Fig.17 (d) is the pigskin after bending. Fig.17 (e) is the pigskin that has been rinsed. Fig.15 It can be seen that the porous foam hydrogel on the pig skin in Example 2 remains in its original shape after being subjected to various forces such as stretching, twisting and bending, without any cracks or falling off; Fig.16 It can be seen that in Comparative Example 5, cracks appeared on the surface of the hydrogel on the pig skin after being bent and twisted, indicating that the anti-bending performance of the porous foam gel is much better than that of the non-foamed hydrogel; Fig.17 It can be seen that in Comparative Example 9, the porous foam on the pigskin has a good surface after being bent and twisted.

[0092] Experimental Example 5

[0093] The solution to be foamed in Example 4 was extruded onto dry pigskin through the foaming device provided in Example 1, and then covered with a glass plate, and then irradiated with ultraviolet light for 5 minutes, 10 minutes and 15 minutes to crosslink it, forming a porous foam hydrogel on the pigskin; the solution to be foamed in Comparative Example 5 was directly extruded onto dry pigskin without foaming, and then extruded and foamed, and then covered with a glass plate, and then irradiated with ultraviolet light for 3 minutes, 5 minutes and 10 minutes to crosslink it, forming a hydrogel on the pigskin. The shear stress of the hydrogel was tested according to the following method:

[0094] The lap shear test was carried out on a universal testing machine using a tensile fixture with one clamp holding the pigskin and the other clamp holding the glass plate. The results are shown in Fig.18 and Fig.19 , Fig.18 is the lap shear stress-strain diagram of the porous foam hydrogel prepared in Example 4, Fig.19 is the lap shear stress-strain diagram of the hydrogel prepared in Comparative Example 5. Fig.18 and Fig.19It can be seen that the porous foam gel prepared in Example 4 has significant changes within the illumination range, and the shear stress can reach nearly 25 kPa after 15 minutes of illumination time, indicating that the shear stress of the porous foam gel has a larger regulation range and can obtain a higher shear stress; the shear stress of the hydrogel on the pig skin in Comparative Example 5 has basically no significant changes at 3 minutes, 5 minutes, and 10 minutes, and can reach about 18 to 23 kPa.

[0095] The foaming solution of Example 2 was extruded onto dry pigskin through the foaming device provided in Example 1 to form foams, and then covered with a glass plate. The foaming solution was then irradiated with ultraviolet light for 10 minutes to crosslink the solution, thereby forming a porous foam hydrogel on the pigskin. The foaming solution of Comparative Example 9 was foamed and then injected into dry pigskin through a needle end to cover a glass plate. The solution was then irradiated with ultraviolet light for 10 minutes to crosslink and cure the solution, thereby obtaining a porous foam hydrogel. The bonding tensile stress-strain curve of the hydrogel sample was measured using a universal testing machine. The results are shown in FIG. Fig. 20 , Fig. 20 Pigskin-glass lap test results provided for Example 2 and Comparative Example 9 are Fig. 20 It can be seen that the adhesion of the porous foam prepared in the present application is much greater than that of the porous foam obtained by the method of Comparative Example 9.

[0096] The solution to be foamed in Example 2 is directly extruded between two pieces of pigskin through the foaming device provided in Example 1, and the pores between the two pieces of pigskin are filled with the extruded hydrogel through a small spoon, and then cross-linked by ultraviolet light for 10 minutes to form a porous foam hydrogel on the pigskin; the foaming solution of Comparative Example 9 is foamed and injected between the two pieces of pigskin through a needle end, and the pores between the two pieces of pigskin are filled with the extruded hydrogel through a small spoon, and cross-linked and cured by ultraviolet light for 10 minutes to obtain a porous foam hydrogel. The bonding tensile stress-strain curve of the hydrogel sample is measured using a universal testing machine. The results are shown in FIG. Fig.21 , Fig.21 The pigskin-pigskin overlap test results provided for Example 2 and Comparative Example 9 are as follows: Fig.21 It can be seen that the adhesion of the porous foam prepared in the present application is much greater than that of the porous foam obtained by the method of Comparative Example 9.

[0097] Embodiment 13

[0098] 5g of gelatin was mixed with 50mL of PBS phosphate buffered saline and stirred on a 60°C hot plate until dissolved to form a 10% (w / v) gelatin solution. Then, 4mL of methacrylic anhydride (MA) was added to the gelatin solution at a rate of 0.5mL / min. After the reaction was completed, PBS phosphate buffered saline was added to the solution and the solution was diluted to 5 times the volume. Dialysis was performed with deionized water at 40°C using a dialysis membrane to maximize the removal of unreacted by-products. After the dialysis was completed, freeze drying was performed to obtain methacrylated gelatin (GelMA). Freeze-dried GelMA was dissolved in PBS solution to prepare 10wt%, 15wt% and 20wt% solutions respectively, and then 0.5wt% of photoinitiator phenyl (2,4,6-trimethylbenzoyl) lithium phosphate (LAP) was added to obtain a solution to be foamed; the solution to be foamed was foamed by the foaming device provided in Example 1, and then cross-linked and cured under the action of an ultraviolet emitter, wherein the mesh number of the sieve in the foaming device was 300 meshes, and a porous foam hydrogel was obtained.

[0099] See also Fig. 22 , Fig. 22 is a scanning electron microscope photograph of the porous foam hydrogel prepared in Example 13 of the present application, wherein: Fig. 22 (a) is a scanning electron microscope photograph of 10 wt% photo-crosslinked gelatin, irradiated with UV light for 10 min. (b) is a scanning electron microscope photograph of 15 wt% photo-crosslinked gelatin, irradiated with UV light for 10 min. (c) is a scanning electron microscope photograph of 20 wt% photo-crosslinked gelatin, irradiated with UV light for 10 min. (d) is a scanning electron microscope photograph of 10 wt% photo-crosslinked gelatin, irradiated with UV light for 15 min. (e) is a scanning electron microscope photograph of 15 wt% photo-crosslinked gelatin, irradiated with UV light for 15 min. (f) is a scanning electron microscope photograph of 20 wt% photo-crosslinked gelatin, irradiated with UV light for 15 min. Fig. 22 It can be seen that the porous foam hydrogel prepared by the method provided by the present invention has large porosity and good connectivity between pores.

[0100] Embodiment 14

[0101] First, prepare a gelatin solution: weigh 1 g of gelatin particles in 10 mL of deionized water, heat and stir at 50°C until the gelatin particles are completely dissolved, and obtain a gelatin solution with a mass / volume fraction of 10%;

[0102] Preparation of crosslinker solution: weigh 0.01 g of 4-morpholineethanesulfonic acid (MES) and add it into 10 mL of water to dissolve it completely, then add 0.5 mmol of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (EDC) and 0.2 mmol of N-hydroxysuccinimide (NHS) in sequence, and stir until the reagents are completely dissolved to obtain the original concentration crosslinker solution (defined as 1 concentration crosslinker solution). In the experiment, the original crosslinker solution was diluted to test different crosslinker parameters;

[0103] The gelatin solution and the cross-linking agent solution were mixed in a centrifuge tube and stirred at high speed for 20 seconds to obtain a gelatin cross-linking agent mixed solution. The mixed solution was extruded and foamed through the foaming device provided in Example 1, and the foam was allowed to stand for 15 minutes to allow a cross-linking reaction to occur, thereby obtaining a porous foam hydrogel.

[0104] See also Fig.23 , Fig.23 is a scanning electron microscope photograph of the porous foam hydrogel prepared in Example 14 of the present invention, wherein: Fig.23 (a) is a scanning electron microscope photo of a porous foam hydrogel obtained from a 3 / 8 concentration cross-linking solution. Fig.23 (b) is a scanning electron microscope photo of a porous foam hydrogel obtained from a 5 / 8 concentration cross-linking solution. Fig.23 (c) is a scanning electron microscope photo of a porous foam hydrogel obtained from a cross-linking solution with a concentration of 1. Fig.23 It can be seen that the porous foam hydrogel prepared by the method provided by the present invention has large porosity and good connectivity between pores.

[0105] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a porous foam hydrogel, comprising: mixing a hydrogel precursor with a cross-linking agent to obtain a mixed solution; The mixed solution is mixed with gas and then foamed through a screen, and the obtained foam is cross-linked and solidified to obtain a porous foam hydrogel; The aperture of the sieve is 100-1000 meshes.

2. The preparation method according to claim 1, characterized in that: The hydrogel precursor is selected from one or more of silk fibroin solution, gelatin solution, alginate solution, hyaluronic acid solution, collagen solution, chitosan solution, functionalized silk fibroin solution, functionalized gelatin solution, functionalized alginate solution, functionalized hyaluronic acid solution, functionalized collagen solution, and functionalized chitosan solution.

3. The preparation method according to claim 1, characterized in that: The concentration of the hydrogel precursor is 1 wt% to 30 wt%.

4. The preparation method according to claim 1, characterized in that: The cross-linking agent is a photoinitiator, and the cross-linking curing is cross-linking curing under light conditions.

5. The preparation method according to claim 4, characterized in that: The photoinitiator is selected from lithium phenyl-2,4,6-trimethylbenzoylphosphonate (LAP), IRGACURE 2959, IRGACURE 784, safranineO Safranine-based, eosin Y, Ru(bpy)3 2+ , zinc tetraphenylporphyrin (ZnTPP) or TPO.

6. The preparation method according to claim 1, characterized in that: The cross-linking agent includes 4-morpholineethanesulfonic acid, a mixture of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide, glutaraldehyde, an epoxy compound or carbodiimide, and the cross-linking curing is cross-linking curing at room temperature.

7. The preparation method according to any one of claims 4 to 6, characterized in that: The cross-linking and curing time is 5s to 20min.

8. The preparation method according to claim 7, characterized in that: The amount of the cross-linking agent used is 0.1 wt% to 10 wt% of the hydrogel precursor.

9. A device for preparing a porous foam hydrogel, comprising: A hydrogel precursor storage unit storing a hydrogel precursor; a cross-linking agent storage unit for storing the cross-linking agent; A foaming unit whose inlet is connected to the hydrogel precursor storage unit and the crosslinking agent storage unit comprises a gas-liquid mixing chamber, a screen connected to the gas-liquid mixing chamber, and an extrusion device for compressing the gas-liquid mixing chamber.

10. The preparation device according to claim 9, characterized in that: Also includes: A light irradiation unit is used for light curing the foam extruded from the bubble unit.

Citation Information

Patent Citations

  • Foaming soap dispensers

    CN105935269A

  • A liquid oral care product provided with foam by shaped container

    CN114948768A

  • Hydrogel foam material capable of being used for 3D printing as well as preparation method and application of hydrogel foam material

    CN115120779A

  • Bubbling injector

    CN210384539U

  • Fabricating Scaffolds and Other Cell-Growth Structures Using Microfluidics to Culture Biological Samples