Long-life soft cross-linked polyolefin material as well as preparation method and application thereof
By combining grafting component A and catalytic component B, a long-life, flexible cross-linked polyolefin material was prepared, solving the problems of hardening and embrittlement and reduced electrical properties of traditional materials, and improving the material's flexibility and aging resistance.
Patent Information
- Application Number
- CN202410998628.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-24
AI Technical Summary
Traditional cross-linked polyolefin materials are prone to hardening and embrittlement during long-term use, affecting their service life and performance. Furthermore, rubber blending methods lead to reduced electrical properties and plasticizer migration, affecting stability.
A grafted component A and a catalytic component B with a weight ratio of 90-95:5-10 were used. The grafted component A included VLLDPE, rubber, ethylene-octene copolymer, silane crosslinking agent, etc., while the catalytic component B included ethylene-vinyl acetate copolymer, antioxidant and catalyst. Crosslinked polyolefin materials were prepared by twin-screw extruder.
It improves the flexibility and aging resistance of cross-linked polyolefin materials, extends their service life, and maintains excellent electrical properties.
Smart Images

Figure BDA0004960954370000061 
Figure BDA0004960954370000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyolefin materials, and in particular to a long-life soft cross-linked polyolefin material and a preparation method and application thereof. Background Art
[0002] Cross-linked polyolefin materials are widely used in cable sheaths and other fields due to their excellent electrical properties, heat resistance and mechanical properties. However, traditional cross-linked polyolefin materials are prone to hardening, embrittlement and other problems during long-term use, which affects their service life and performance. At present, in order to improve the softness of cross-linked polyolefin materials, they are usually blended with rubber and plasticizers are added to the rubber to reduce the hardness of cross-linked polyolefins. However, this method will lead to a decrease in the electrical properties of the cross-linked polyolefin materials, and the plasticizer is easy to migrate, affecting the long-term stability of the cross-linked polyolefin materials. In addition, due to the presence of unsaturated bonds in the rubber, it is easily attacked by oxygen free radicals under high temperature conditions, which affects the service life of the cross-linked polyolefin materials. Summary of the invention
[0003] In order to improve the aging resistance of cross-linked polyolefin, the present invention provides a long-life soft cross-linked polyolefin material and a preparation method and application thereof.
[0004] The first aspect of the present invention provides a long-life soft cross-linked polyolefin material, which adopts the following technical scheme: a long-life soft cross-linked polyolefin material, comprising a grafted A component and a catalytic B component in a weight ratio of 90-95:5-10, wherein the total amount of the grafted A component and the B component is 100; The grafting A component raw materials include, by weight: 15-40 parts of VLLDPE, 30-50 parts of rubber, 30-45 parts of ethylene-octene copolymer, 2-8 parts of silane crosslinking agent, 0.5-1.5 parts of initiator, 0.5-2 parts of lubricant, 1-4 parts of first antioxidant, and 0.5-3 parts of metal oxide; The catalyst B component raw materials include, by weight: 100 parts of ethylene-vinyl acetate copolymer, 3-7 parts of a second antioxidant, 5-12 parts of a third antioxidant, and 5-10 parts of a catalyst.
[0005] Preferably, the grafting A component raw materials include, by weight: 20-30 parts of VLLDPE, 35-45 parts of rubber, 35-45 parts of ethylene-octene copolymer, 3-6 parts of silane crosslinking agent, 0.5-1.5 parts of initiator, 0.5-2 parts of lubricant, 1-4 parts of first antioxidant, and 0.5-3 parts of metal oxide; The catalyst B component raw materials include, by weight: 100 parts of ethylene-vinyl acetate copolymer, 4-7 parts of a second antioxidant, 6-10 parts of a third antioxidant, and 5-10 parts of a catalyst.
[0006] Preferably, the rubber includes one or both of EVM rubber and HNBR rubber.
[0007] Preferably, the weight ratio of the EVM rubber to the HNBR rubber is 1:(1-2).
[0008] Preferably, the silane crosslinking agent comprises methyltrimethoxysilane and vinyltrimethoxysilane in a weight ratio of 1:(1-3).
[0009] Preferably, the metal oxide is zinc oxide.
[0010] Preferably, the first antioxidant is antioxidant 1010.
[0011] Preferably, the second antioxidant is allylphenol, and the third antioxidant is 2-methoxy-4-allylphenol.
[0012] The second aspect of the present invention provides a method for preparing a long-life soft cross-linked polyolefin material, comprising the following preparation steps: preparing a grafted A component, mixing each raw material evenly according to a formula ratio, kneading and granulating, and then drying to obtain the grafted A component; preparing a catalytic B component, mixing each raw material evenly according to a formula ratio, extruding through a twin-screw extruder, granulating, and drying to obtain the catalytic B component, and mixing the grafted A component and the catalytic B component in a weight ratio to obtain a cross-linked polyolefin material.
[0013] The third aspect of the present invention provides an application of a long-life soft cross-linked polyolefin material, wherein the cross-linked polyolefin is used to prepare cable materials and wire cable materials.
[0014] In summary, the present invention has the following beneficial effects: VLLDPE is an ultra-low density polyethylene with a moderate degree of branching, containing more short branches and more tertiary carbon atoms on the main chain. Therefore, VLLDPE has a high reactivity with silane crosslinkers, ethylene-octene copolymers, etc. The molecular chains are connected by Si-O-Si crosslinking bonds, and the side chains provided by the octene of the ethylene-octene copolymer serve as the active points of the crosslinking reaction, which increases the length of the molecular chains between the crosslinking points of the crosslinking network, makes it easy for the molecular chain segments to slip relative to each other during stretching, increases the ductility of the material, and improves the elongation at break. In addition, when the rubber is a mixture of one or two of EVM rubber and HNBR rubber, its combination with ethylene-octene copolymer and ethylene-vinyl acetate copolymer increases the upper limit temperature of the use of the crosslinked polyolefin material, thereby improving the aging resistance of the crosslinked polyolefin material. DETAILED DESCRIPTION
[0015] The present invention is further described in detail below with reference to the embodiments.
[0016] The raw materials used in the examples and comparative examples of the present application are all commercially available.
[0017] In the examples and comparative examples of the present application, dicumyl peroxide is used as the initiator; The catalyst is dibutyltin dilaurate; The lubricant is silicone; The melt index of VLLDPE is 1.0g / 10min and the density is 0.888g / cm 3 , purchased from DuPont Dow.
[0018] Example 1 A method for preparing a long-life soft cross-linked polyolefin material comprises the following steps: S1. Preparation of grafted component: 15 kg of VLLDPE, 30 kg of EVM rubber, 30 kg of ethylene-octene copolymer, 2 kg of silane crosslinker, 0.5 kg of dicumyl peroxide, 0.5 kg of silicone, 1 kg of antioxidant 1010 and 0.5 kg of zinc oxide were mixed in a mixer, granulated, dehydrated in a dehydrator and dried to obtain grafted component A; wherein the silane crosslinker comprises methyltrimethoxysilane and vinyltrimethoxysilane in a weight ratio of 1:1; S2, preparation of catalytic component: 100kg of ethylene-vinyl acetate copolymer, 3-7kg of allyl phenol, 5-12kg of 2-methoxy-4-allyl phenol, and 5-10kg of dibutyltin dilaurate are uniformly mixed, and then extruded and granulated by a twin-screw extruder to obtain catalytic component B, wherein the feeding section temperature of the twin-screw extruder is 120-130°C, the compression section temperature is 135-155°C, the homogenization section temperature is 160-175°C, and the head temperature is 165-185°C; S3. According to a total amount of 100 kg, 90 kg of the grafted A component and 10 kg of the catalytic B component are mixed and packaged to obtain a cross-linked polyolefin material.
[0019] Example 2 A method for preparing a long-life soft cross-linked polyolefin material comprises the following steps: S1. Preparation of grafted component: 20 kg of VLLDPE, 35 kg of EVM rubber, 35 kg of ethylene-octene copolymer, 3 kg of silane crosslinker, 0.6 kg of dicumyl peroxide, 0.7 kg of silicone, 1 kg of antioxidant 1010 and 1 kg of zinc oxide were mixed in a mixer, granulated, dehydrated in a dehydrator and dried to obtain grafted component A; wherein the silane crosslinker comprises methyltrimethoxysilane and vinyltrimethoxysilane in a weight ratio of 1:1; S2, preparation of catalytic component: 100kg of ethylene-vinyl acetate copolymer, 4kg of allylphenol, 6kg of 2-methoxy-4-allylphenol and 6kg of dibutyltin dilaurate were mixed evenly, and then extruded and granulated by twin screw extruder to obtain catalytic component B, wherein the feeding section temperature of the twin screw extruder was 120-130°C, the compression section temperature was 135-155°C, the homogenization section temperature was 160-175°C, and the die head temperature was 165-185°C; S3. According to a total amount of 100 kg, 95 kg of grafted component A and 5 kg of catalytic component B are mixed and packaged to obtain a cross-linked polyolefin material.
[0020] Example 3 A method for preparing a long-life soft cross-linked polyolefin material comprises the following steps: S1. Preparation of grafted component: 25 kg of VLLDPE, 40 kg of EVM rubber, 40 kg of ethylene-octene copolymer, 5 kg of silane crosslinker, 1.0 kg of dicumyl peroxide, 1.2 kg of silicone, 3 kg of antioxidant 1010, and 2 kg of zinc oxide were mixed in a mixer, granulated, dehydrated in a dehydrator, and dried to obtain grafted component A; wherein the silane crosslinker comprises methyltrimethoxysilane and vinyltrimethoxysilane in a weight ratio of 1:1; S2, preparation of catalyst component: 100kg of ethylene-vinyl acetate copolymer, 5kg of allyl phenol, 8kg of 2-methoxy-4-allyl phenol and 7kg of dibutyltin dilaurate were mixed evenly, and then extruded and granulated by twin screw extruder to obtain catalyst component B, wherein the feeding section temperature of the twin screw extruder was 120-130°C, the compression section temperature was 135-155°C, the homogenization section temperature was 160-175°C, and the die head temperature was 165-185°C; S3. According to a total amount of 100 kg, 90 kg of the grafted A component and 10 kg of the catalytic B component are mixed and packaged to obtain a cross-linked polyolefin material.
[0021] Example 4 A method for preparing a long-life soft cross-linked polyolefin material comprises the following steps: S1. Preparation of grafted component: 30 kg of VLLDPE, 45 kg of EVM rubber, 42 kg of ethylene-octene copolymer, 6 kg of silane crosslinker, 1 kg of dicumyl peroxide, 1.5 kg of silicone, 3 kg of antioxidant 1010, and 2.5 kg of zinc oxide were mixed in a mixer, granulated, dehydrated in a dehydrator, and dried to obtain grafted component A; wherein the silane crosslinker comprises methyltrimethoxysilane and vinyltrimethoxysilane in a weight ratio of 1:1; S2, preparation of catalytic component: 100kg of ethylene-vinyl acetate copolymer, 6kg of allyl phenol, 10kg of 2-methoxy-4-allyl phenol, and 8kg of dibutyltin dilaurate were mixed uniformly, and then extruded and granulated by a twin-screw extruder to obtain catalytic component B, wherein the feeding section temperature of the twin-screw extruder was 120-130°C, the compression section temperature was 135-155°C, the homogenization section temperature was 160-175°C, and the die head temperature was 165-185°C; S3. According to a total amount of 100 kg, 90 kg of the grafted A component and 10 kg of the catalytic B component are mixed and packaged to obtain a cross-linked polyolefin material.
[0022] Example 5 A method for preparing a long-life soft cross-linked polyolefin material comprises the following steps: S1. Preparation of grafted component: 40 kg of VLLDPE, 50 kg of EVM rubber, 45 kg of ethylene-octene copolymer, 8 kg of silane crosslinker, 1.5 kg of dicumyl peroxide, 2 kg of silicone, 4 kg of antioxidant 1010 and 3 kg of zinc oxide were mixed in a mixer, granulated, dehydrated in a dehydrator and dried to obtain grafted component A; wherein the silane crosslinker comprises methyltrimethoxysilane and vinyltrimethoxysilane in a weight ratio of 1:1; S2, preparation of catalyst component: 100kg of ethylene-vinyl acetate copolymer, 7kg of allylphenol, 12kg of 2-methoxy-4-allylphenol and 10kg of dibutyltin dilaurate were mixed evenly, and then extruded and granulated by twin screw extruder to obtain catalyst component B, wherein the feeding section temperature of the twin screw extruder was 120-130°C, the compression section temperature was 135-155°C, the homogenization section temperature was 160-175°C, and the die head temperature was 165-185°C; S3. According to a total amount of 100 kg, 90 kg of the grafted A component and 10 kg of the catalytic B component are mixed and packaged to obtain a cross-linked polyolefin material.
[0023] Example 6 A method for preparing a long-life soft cross-linked polyolefin material, which is different from Example 3 in that the silane cross-linking agent includes methyltrimethoxysilane and vinyltrimethoxysilane in a weight ratio of 1:2, that is, the content of methyltrimethoxysilane is 1.67kg and the content of vinyltrimethoxysilane is 3.33kg, and the rest is the same as in Example 3.
[0024] Example 7 A method for preparing a long-life soft cross-linked polyolefin material, which is different from Example 3 in that the silane cross-linking agent includes methyltrimethoxysilane and vinyltrimethoxysilane in a weight ratio of 1:3, that is, the content of methyltrimethoxysilane is 1.25kg and the content of vinyltrimethoxysilane is 3.75kg, and the rest is the same as in Example 3.
[0025] Example 8 A method for preparing a long-life soft cross-linked polyolefin material, which is different from Example 3 in that only vinyltrimethoxysilane is used as the silane cross-linking agent, and the rest is the same as Example 3.
[0026] Example 9 A method for preparing a long-life soft cross-linked polyolefin material is different from Example 3 in that only methyltrimethoxysilane is used as the silane cross-linking agent, and the rest is the same as Example 3.
[0027] Example 10 A method for preparing a long-life soft cross-linked polyolefin material, which is different from Example 3 in that the silane cross-linking agent includes γ-aminopropyltriethoxysilane and vinyltrimethoxysilane in a weight ratio of 1:1, and the rest is the same as Example 3.
[0028] Embodiment 11 A method for preparing a long-life soft cross-linked polyolefin material, which is different from Example 3 in that the rubber is HNBR rubber, and the rest is the same as Example 3.
[0029] Example 12 A method for preparing a long-life soft cross-linked polyolefin material, which is different from Example 3 in that the rubber is a mixture of EVM rubber and HNBR rubber, and the weight ratio of EVM rubber to HNBR rubber is 1:1, that is, 20kg of EVM rubber and 20kg of HNBR rubber, and the rest is the same as Example 3.
[0030] Comparative Example 12 A method for preparing a long-life soft cross-linked polyolefin material, which is different from Example 3 in that the rubber is a mixture of EPDM rubber and HNBR rubber, and the weight ratio of EPDM rubber to HNBR rubber is 1:1, that is, 20 kg of EPDM rubber and 20 kg of HNBR rubber, and the rest is the same as Example 3.
[0031] Embodiment 13 A method for preparing a long-life soft cross-linked polyolefin material, which is different from Example 3 in that the rubber is a mixture of EVM rubber and HNBR rubber, and the weight ratio of EVM rubber to HNBR rubber is 1:2, that is, 13.3 kg of EVM rubber and 26.7 kg of HNBR rubber, and the rest is the same as Example 3.
[0032] Comparative Example 1 A method for preparing a long-life soft cross-linked polyolefin material, which is different from Example 12 in that an equal amount of LLDPE is used instead of VLLDPE, wherein the melt index of LLDPE is 1.7-2.3 g / 10 min, and the density is 0.918-0.922 g / cm 3 , the rest are the same as Example 12.
[0033] Comparative Example 2 A method for preparing a long-life soft cross-linked polyolefin material, which is different from Example 12 in that: 10kg of VLLDPE, 25kg of rubber, 25kg of ethylene-octene copolymer, and 1kg of silane cross-linking agent are included in the grafted A component; the rubber is a mixture of EVM rubber and HNBR rubber, the weight ratio of EVM rubber to HNBR rubber is 1:1, the silane cross-linking agent includes methyltrimethoxysilane and vinyltrimethoxysilane in a weight ratio of 1:1, and the rest are the same as Example 12.
[0034] Comparative Example 3 A method for preparing a long-life soft cross-linked polyolefin material, which is different from Example 12 in that: 45kg of VLLDPE, 55kg of rubber, 50kg of ethylene-octene copolymer, 10kg of silane cross-linking agent, and 2kg of diisopropylbenzene peroxide are included in the grafted A component; the rubber is a mixture of EVM rubber and HNBR rubber, the weight ratio of EVM rubber to HNBR rubber is 1:1, the silane cross-linking agent includes methyltrimethoxysilane and vinyltrimethoxysilane in a weight ratio of 1:1, and the rest are the same as Example 12.
[0035] Performance Testing The cross-linked polyolefin cable materials obtained in the above embodiments, comparative embodiments and comparative examples were made into test samples with a thickness of 1 mm, and naturally placed under ambient temperature conditions of 25° C. and relative humidity of 65% for 120 h, and then the thermal life performance, hardness, tensile strength and elongation at break were tested. The thermal life of the cable insulation and sheath was evaluated by the methods of GB / T 11026.1-2016 and GB / T 11026.2-2012. The performance selected for life judgment was the elongation at break retention rate, and the end point was 50%. The tensile strength and elongation at break were tested according to the relevant provisions of GB / T1040, and the test results are shown in Table 1.
[0036] Table 1 Performance test results of cross-linked polyolefin as cable material From the above table, we can see that: After the contents of the raw materials in the grafted A component and the catalytic B component were changed in Examples 1-5 of the present application, the hardness of the cross-linked polyolefin materials obtained in Examples 1-5 was 78-82 Shore A, and the elongation at break was greater than or equal to 440%. It can be seen that the cross-linked polyolefin materials obtained in Examples 1-5 of the present application have good softness, and after the cross-linked polyolefin materials in Examples 1-5 of the present application were subjected to an air heat aging test at 180°C×168h, the elongation at break of the cross-linked polyolefin materials was still greater than or equal to 410%, and the tensile strength was greater than 15MPa. It can be seen that the cross-linked polyolefin materials obtained in Examples 1-5 of the present application have good aging resistance and a long service life.
[0037] Compared with Example 3, when the weight ratio of methyltrimethoxysilane and vinyltrimethoxysilane is changed from 1:1 to 1:2 or 1:3, the tensile strength and elongation at break of the cross-linked polyolefin material obtained in Example 6-7 are increased compared with those in Example 3. It can be seen that when the weight ratio of methyltrimethoxysilane and vinyltrimethoxysilane is in the range of 1:1-3, the aging resistance and mechanical properties of the cross-linked polyolefin material can be effectively improved.
[0038] Compared with Example 3, when the silane cross-linking agent only uses vinyltrimethoxysilane or methyltrimethoxysilane, the hardness of the cross-linked polyolefin material obtained in Example 8-9 increases and the elongation at break decreases. It can be seen that the softness of the cross-linked polyolefin material is reduced. After the air heat aging test of 180℃×168h, the elongation at break and the tensile strength of the cross-linked polyolefin material obtained in Example 8-9 are significantly reduced compared with Example 3. This can further illustrate that when the silane cross-linking agent uses a mixture of vinyltrimethoxysilane and methyltrimethoxysilane, the cross-linked polyolefin material obtained is not only softer, but also has better aging resistance and a long service life.
[0039] Compared with Example 3, when the silane crosslinker is a mixture of γ-aminopropyltriethoxysilane and vinyltrimethoxysilane, the hardness of the cross-linked polyolefin material obtained in Example 10 is increased compared with that in Example 3, and the tensile strength and elongation at break are reduced compared with those in Example 3. After the aging resistance test, the retention rates of the elongation at break and the tensile strength are also significantly reduced compared with those in Example 3. It can be seen that when the content and type of other raw materials remain unchanged, the silane crosslinker using a mixture of methyltrimethoxysilane and vinyltrimethoxysilane can effectively improve the softness and aging resistance of the cross-linked polyolefin material.
[0040] Compared with Example 3, when the rubber usage is the same, when the rubber is a mixture of EVM rubber and HNBR rubber, the hardness of the cross-linked polyolefin material obtained in Example 12-13 is reduced and the elongation at break is increased, that is, the softness of the cross-linked polyolefin obtained in Example 12-13 is improved compared with that in Example 3, and after the aging resistance test, the cross-linked polyolefin material obtained in Example 12-13 also has excellent aging resistance. It can be seen that when the rubber is a mixture of EVM rubber and HNBR rubber, the performance of the cross-linked polyolefin obtained is better than that of EVN rubber or HNBR rubber alone.
[0041] Comparative Example 12 Compared with Example 12, when EPDM rubber is used instead of EVM rubber, the softness and aging resistance of the cross-linked polyolefin material obtained in Comparative Example 12 are lower than those in Example 12. It can be seen that the combination of EVM rubber and HNBR rubber can effectively improve the softness and aging resistance of the cross-linked polyolefin material.
[0042] Compared with Example 12, when an equal amount of LLDPE is used instead of VLLDPE, the softness, mechanical properties and aging resistance of the cross-linked polyolefin material obtained in Comparative Example 1 are all lower than those in Example 12. It can be seen that after the base resin is selected as VLLDPE, the softness and aging resistance of the cross-linked polyolefin material can be effectively guaranteed.
[0043] Compared with Example 12, when the contents of VLLDPE, rubber, ethylene-octene copolymer and silane crosslinking agent in Comparative Example 2 are lower than the limits of the present application, the hardness of the cross-linked polyolefin material obtained in Comparative Example 2 increases, and it can be seen that the softness of the cross-linked polyolefin material decreases. After the aging resistance test, the elongation at break and the tensile strength retention rate of the cross-linked polyolefin material decrease rapidly, and the aging resistance is reduced.
[0044] Compared with Example 3, when the content of VLLDPE, rubber, ethylene-octene copolymer and silane crosslinking agent in Comparative Example 3 exceeds the limits of the present application, the hardness of the cross-linked polyolefin material obtained in Comparative Example 3 is reduced and it is more easily deformed. The cross-linked polyolefin material has better softness. However, after the aging resistance test, the elongation at break and the tensile strength of the cross-linked polyolefin material in Comparative Example 3 decrease rapidly. It can be seen that the aging resistance in Comparative Document 3 is greatly reduced. This further illustrates that when the components in the present application are within the range specified in the present application, the cross-linked polyolefin material has good softness and aging resistance.
[0045] The embodiments of this specific implementation method are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A long-life soft cross-linked polyolefin material, characterized in that: The invention comprises a grafting component A and a catalytic component B in a weight ratio of 90-95:5-10, wherein the total amount of the grafting component A and the component B is 100; The grafting A component raw materials include, by weight: 15-40 parts of VLLDPE, 30-50 parts of rubber, 30-45 parts of ethylene-octene copolymer, 2-8 parts of silane crosslinking agent, 0.5-1.5 parts of initiator, 0.5-2 parts of lubricant, 1-4 parts of first antioxidant, and 0.5-3 parts of metal oxide; The catalyst B component raw materials include, by weight: 100 parts of ethylene-vinyl acetate copolymer, 3-7 parts of a second antioxidant, 5-12 parts of a third antioxidant, and 5-10 parts of a catalyst.
2. The long-life soft cross-linked polyolefin material according to claim 1, characterized in that: The grafting A component raw materials include, by weight: 20-30 parts of VLLDPE, 35-45 parts of rubber, 35-45 parts of ethylene-octene copolymer, 3-6 parts of silane crosslinking agent, 0.5-1.5 parts of initiator, 0.5-2 parts of lubricant, 1-4 parts of first antioxidant, and 0.5-3 parts of metal oxide; The catalyst B component raw materials include, by weight: 100 parts of ethylene-vinyl acetate copolymer, 4-7 parts of a second antioxidant, 6-10 parts of a third antioxidant, and 5-10 parts of a catalyst.
3. A long-life soft cross-linked polyolefin material according to claim 1 or 2, characterized in that: The rubber includes one or both of EVM rubber and HNBR rubber.
4. The long-life soft cross-linked polyolefin material according to claim 3, characterized in that: The weight ratio of the EVM rubber to the HNBR rubber is 1:(1-2).
5. A long-life soft cross-linked polyolefin material according to claim 1 or 2, characterized in that: The silane crosslinking agent includes methyltrimethoxysilane and vinyltrimethoxysilane in a weight ratio of 1:(1-3).
6. The long-life soft cross-linked polyolefin material according to claim 1, characterized in that: The metal oxide is zinc oxide.
7. A long-life soft cross-linked polyolefin material according to claim 1 or 2, characterized in that: The first antioxidant is antioxidant 1010.
8. A long-life soft cross-linked polyolefin material according to claim 1 or 2, characterized in that: The second antioxidant is allylphenol, and the third antioxidant is 2-methoxy-4-allylphenol.
9. A method for preparing the long-life soft cross-linked polyolefin material according to any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: preparing a grafted component A, mixing various raw materials evenly according to a formula ratio, kneading and granulating, and then drying to obtain the grafted component A; preparing a catalytic component B, mixing various raw materials evenly according to a formula ratio, extruding through a twin-screw extruder, granulating, and drying to obtain the catalytic component B; and mixing the grafted component A and the catalytic component B according to a weight ratio to obtain a cross-linked polyolefin material.
10. An application of the long-life soft cross-linked polyolefin material according to claim 9, characterized in that: The cross-linked polyolefin is used for preparing cable materials and wire cable materials.
Citation Information
Patent Citations
Thermal stable polyoxymethylene containing high-efficiency anti-oxidant and method for producing the same
CN101508819A
Silane self-crosslinking halogen-free low-smoke flame-retardant elastic material and preparation method thereof
CN102731917A
Silane self-crosslinked polyolefin flexible insulation cable material and preparation method thereof
CN102936369A
Soft transparent silane cross-linked polyethylene insulated material and preparation method thereof
CN103642108A
Silane crosslinking halogen-free flame retardant polyolefin composite material and preparation method thereof