Cable sheath material with high wear resistance and high mechanical strength and preparation method thereof

By using a combination of chlorosulfonated polyethylene and wollastonite nanotubes in the cable sheath, combined with electrostatic adsorption and vulcanization crosslinking technology, the cable is solved due to tension and resistance in coal mines, and the cable is significantly improved The tear resistance and wear resistance extend the service life.

CN118895027AActive Publication Date: 2024-11-05JIANGSU SHANGSHANG CABLE GRP NEW MATERIAL CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411050430.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-05
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

During the use of existing cable sheaths in coal mines, they are easily damaged due to internal tension and ground resistance, resulting in a shortened service life, especially when towing streamers in coal seams with inclinations greater than 30°.

Method used

Using high wear-resistant and high mechanical strength cable sheath material, by using chlorosulfonated polyethylene as the base material, and adding wollastonite nanotubes, zinc oxide, plasticizer, lead stearate, and anti-aging in the additives The agent, flame retardant and surfactant improve the tear resistance and wear resistance of the cable sheath through electrostatic adsorption and vulcanization cross-linking.

Benefits of technology

It significantly extends the service life of the cable, can effectively reduce damage in harsh environments of coal mines, adapt to the situation of large inclination streamers, improves the mechanical strength and wear resistance of the cable, and has good application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004974750730000061
    Figure BDA0004974750730000061
  • Figure BDA0004974750730000071
    Figure BDA0004974750730000071
  • Figure BDA0004974750730000072
    Figure BDA0004974750730000072
Patent Text Reader

Abstract

The invention relates to the technical field of insulating materials, and particularly discloses a cable sheath material with high wear resistance and high mechanical strength and a preparation method thereof. The cable sheath material is obtained by mixing an auxiliary agent, 100 parts by weight of chlorosulfonated polyethylene, 3-5 parts by weight of a vulcanizing agent and 2-3.5 parts by weight of a vulcanization accelerator, and the auxiliary agent comprises the following components in parts by weight: 10-15 parts of zinc oxide, 15-30 parts of a plasticizer, 5-10 parts of lead stearate, 3-5 parts of an anti-aging agent, 20-30 parts of a flame retardant, 30-50 parts of white carbon black and 10-15 parts of wollastonite nanotubes. And 10-15 parts of talcum powder. When the cable sheath material is used in cable production, the cable sheath material can fully adapt to the operation condition of a coal mine, the damage to the cable caused by the combined action of internal tension and ground resistance is reduced, the service life of the cable is prolonged, and the cable sheath material has a good application prospect in the mine cable industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of insulating materials, and more specifically, to a cable sheath material with high wear resistance and high mechanical strength and a preparation method thereof. Background Art

[0002] Coal is an important fossil fuel and an important resource for industrial production. Coal mining is mainly carried out in the form of mine operations. In order to fully expand coal production capacity, coal mines generally use high-power coal mining equipment for mining. The cables of high-power coal mining equipment will frequently rub against the well wall during use, and are also easily hit by falling rocks, which requires the cable sheath material to have good wear resistance and tear resistance.

[0003] At present, the cables used in high-power coal mining machines mainly use chlorinated polyethylene as the base material of the cable sheath material, and are mixed after adding vulcanizers, vulcanization accelerators, flame retardants, plasticizers, antioxidants, flame retardants and other additives during the production and processing. The cable sheath material obtained in this way has a certain ability to withstand the friction of the well wall and the collision of falling rocks.

[0004] In view of the above-mentioned related technologies, the inventor believes that although the cable sheath materials currently used in high-power coal mining machines on the market have a certain bearing effect on the friction of the well wall and the collision of falling rocks, in the actual construction process, the coal seam environment will limit the operation of the coal mining equipment towing device, resulting in the use of manual towing. Once the manual towing process encounters a coal seam with an inclination of more than 30°, the cable sheath is easily damaged due to the combined effect of internal tension and ground resistance, which will still seriously affect the service life of the cable. Summary of the invention

[0005] For cables in the related art, once encountering a coal seam with an inclination angle exceeding 30° during the artificial cable dragging process, the cable sheath is easily damaged due to the combined effect of internal tension and ground resistance, which seriously affects the service life of the cable. In order to improve this defect, the present application provides a cable sheath material with high wear resistance and high mechanical strength and a preparation method thereof.

[0006] In the first aspect, the present application provides a cable sheath material with high wear resistance and high mechanical strength, which adopts the following technical solution: A cable sheath material with high wear resistance and high mechanical strength. The cable sheath material is obtained by mixing an auxiliary agent, 100 parts by weight of chlorosulfonated polyethylene, 3-5 parts by weight of a vulcanizing agent, and 2-3.5 parts by weight of a vulcanization accelerator. The auxiliary agent comprises the following components in parts by weight: 10-15 parts of zinc oxide, 15-30 parts of a plasticizer, 5-10 parts of lead stearate, 3-5 parts of an antioxidant, 20-30 parts of a flame retardant, 30-50 parts of white carbon black, 10-15 parts of wollastonite nanotubes, and 10-15 parts of talc.

[0007] By adopting the above technical scheme, compared with the related art, the present application adds wollastonite nanotubes to the auxiliary agent, and adjusts the base material of the cable sheath material from chlorinated polyethylene to chlorosulfonated polyethylene. The composition of wollastonite nanotubes is calcium metasilicate, and the molecules of chlorosulfonated polyethylene contain sulfonic acid groups. There is an electrostatic adsorption effect between the calcium ions in calcium metasilicate and the sulfonic acid groups in chlorosulfonated polyethylene. Therefore, the wollastonite nanotubes have a certain pulling effect on the molecules of chlorosulfonated polyethylene, thereby reinforcing the chlorosulfonated polyethylene and improving the tear resistance of the cable sheath material. At the same time, wollastonite nanotubes also have good hardness and rigidity, which can reduce the scratches of the cable sheath material when the cable sheath material is subjected to friction, thereby improving the wear resistance of the cable sheath material. By using the cable sheath material of the present application in cable production, it can fully adapt to the harsh operating conditions of coal mines. Even if encountering a coal seam with an inclination greater than 30° (the inclination refers to the angle between the coal seam layer and the horizontal plane) during the cable towing process, the damage to the cable caused by the combined effects of internal tension and ground resistance can be fully reduced, thereby extending the service life of the cable, and has good application prospects in the mining cable industry.

[0008] Preferably, the auxiliary agent also includes a surfactant, and the surfactant has a carbon-carbon double bond in its molecule.

[0009] By adopting the above technical scheme, the present application adds a surfactant to the auxiliary agent, and improves the dispersibility of the wollastonite nanotubes by adsorption between the surfactant and the wollastonite nanotubes. After the surfactant is adsorbed on the wollastonite nanotubes, carbon-carbon double bonds are introduced to the surface of the wollastonite nanotubes. Under the action of the vulcanizing agent, the carbon-carbon double bonds can be cross-linked by vulcanization with the chain segments of chlorosulfonated polyethylene, which not only increases the degree of cross-linking by vulcanization of the chlorosulfonated polyethylene, but also improves the bonding between the wollastonite nanotubes and the chlorosulfonated polyethylene, thereby improving the tear resistance of the cable sheath material.

[0010] Preferably, the surfactant comprises sodium oleyl alcohol polyoxyethylene ether sulfonate.

[0011] By adopting the above technical scheme, the specific type of surfactant is selected. The molecule of sodium oleyl alcohol polyoxyethylene ether sulfonate contains sulfonic acid groups and is an anionic surfactant. Compared with non-ionic surfactants, it is easier to adsorb calcium ions on the surface of wollastonite nanotubes. Therefore, it can more fully improve the bonding degree between wollastonite nanotubes and chlorosulfonated polyethylene, and is also more conducive to improving the tear resistance of cable sheath materials.

[0012] Preferably, the amount of sodium oleyl alcohol polyoxyethylene ether sulfonate used is 2.6-3.4% of the weight of the wollastonite nanotubes.

[0013] By adopting the above technical solution, the dosage of sodium oleyl alcohol polyoxyethylene ether sulfonate is optimized, which helps to fully improve the tear resistance and wear resistance of the cable sheath material while saving production costs.

[0014] Preferably, the wollastonite nanotubes are prepared according to the following method: (1) Sodium silicate and calcium nitrate are added to water to prepare a solution, polyethylene glycol is then added to the calcium nitrate solution, and then the sodium silicate solution is added dropwise to the calcium nitrate solution, and stirring is continued during the dropping process, and the calcium nitrate solution is filtered after no more precipitation occurs, and the precipitate obtained by filtration is washed and dried to obtain a nanotube precursor; (2) A nanotube precursor, sodium nitrate, and anhydrous sodium carbonate are mixed in a weight ratio of 1:5:(0.3-0.5) and ground to obtain a mixture; the mixture is heated at 350° C. for 2 h, and the mixture is washed after cooling until the pH of the washing liquid is 7, and the washing residue is dried to obtain wollastonite nanotubes.

[0015] By adopting the above technical scheme, the present application first uses sodium silicate and calcium nitrate to react to generate calcium metasilicate to prepare a nanotube precursor. Then, the nanotube precursor is eroded by sodium carbonate in a sodium nitrate melt, so that the silicon dioxide phase on the surface is reduced, and a wollastonite nanotube with a more dense distribution of surface calcium ions is obtained. With the increase of the density of calcium ion distribution on the surface of the wollastonite nanotube, the wollastonite nanotube can be adsorbed with more molecules of sodium oleyl alcohol polyoxyethylene ether sulfonate, and the bonding degree between the wollastonite nanotube and chlorosulfonated polyethylene is also improved, thereby improving the tear resistance of the cable sheath material.

[0016] Preferably, the nanotube precursor, sodium nitrate and anhydrous sodium carbonate are mixed in a weight ratio of 1:5:0.35, and the amount of sodium oleyl alcohol polyoxyethylene ether sulfonate is 3.8% of the weight of the wollastonite nanotubes.

[0017] By adopting the above technical solution, the ratio of nanotube precursor, sodium nitrate and anhydrous sodium carbonate is optimized, which helps to improve the bonding degree between wollastonite nanotubes and chlorosulfonated polyethylene while saving the amount of anhydrous sodium carbonate.

[0018] Preferably, the nanotube precursor, sodium nitrate and anhydrous sodium carbonate are mixed in a weight ratio of 1:5:0.5, and the amount of sodium oleyl alcohol polyoxyethylene ether sulfonate is 4.2-6.0% of the weight of the wollastonite nanotubes.

[0019] By adopting the above technical solution, the present application optimizes the mixing ratio of nanotube precursor, sodium nitrate and anhydrous sodium carbonate, fully increases the density of calcium ion distribution on the surface of wollastonite nanotubes, and on this basis optimizes the dosage range of sodium oleyl alcohol polyoxyethylene ether sulfonate. With the increase of the adsorption amount of sodium oleyl alcohol polyoxyethylene ether sulfonate, the bonding degree between wollastonite nanotubes and chlorosulfonated polyethylene increases, and the tear resistance of the cable sheath material is improved to a certain extent.

[0020] Preferably, the dosage of the sodium oleyl alcohol polyoxyethylene ether sulfonate is 6.0% of the weight of the wollastonite nanotubes, and the surfactant further comprises oleyl alcohol polyoxyethylene ether.

[0021] By adopting the above technical scheme, the present application uses oleyl alcohol polyoxyethylene ether and oleyl alcohol polyoxyethylene ether sodium sulfonate as surfactants together. The structure of oleyl alcohol polyoxyethylene ether is similar to that of oleyl alcohol polyoxyethylene ether sodium sulfonate, both of which have carbon-carbon double bonds, but oleyl alcohol polyoxyethylene ether does not have sulfonic acid groups and is a nonionic surfactant. When the adsorption of oleyl alcohol polyoxyethylene ether sodium sulfonate reaches a state close to saturation, oleyl alcohol polyoxyethylene ether can be inserted between adjacent oleyl alcohol polyoxyethylene ether sodium sulfonates, reducing the electrostatic repulsion between the sulfonic acid groups and increasing the distribution density of surfactant molecules with double bonds on the surface of wollastonite nanotubes. Both oleyl alcohol polyoxyethylene ether and oleyl alcohol polyoxyethylene ether sodium sulfonate can be cross-linked with chlorosulfonated polyethylene through double bonds under the action of a vulcanizing agent, so oleyl alcohol polyoxyethylene ether further increases the bonding degree between wollastonite nanotubes and chlorosulfonated polyethylene, improving the tear resistance and wear resistance of the cable sheath material.

[0022] Preferably, the amount of oleyl alcohol polyoxyethylene ether used is 28-36% by weight of the sodium oleyl alcohol polyoxyethylene ether sulfonate.

[0023] By adopting the above technical solution, the dosage of oleyl alcohol polyoxyethylene ether is optimized, which helps to fully improve the tear resistance and wear resistance of the cable sheath material while saving production costs.

[0024] In a second aspect, the present application provides a method for preparing a cable sheath material with high wear resistance and high mechanical strength, using the following technical solution.

[0025] A method for preparing a cable sheath material with high wear resistance and high mechanical strength comprises the following steps: (1) Prepare any of the above auxiliary agents and set aside; (2) adding chlorosulfonated polyethylene into an internal mixer and heating it to 70-80°C; (3) Add the additives into an internal mixer and mix for 2-3 minutes; (4) Add the vulcanizing agent and the vulcanization accelerator into the internal mixer and continue to mix for 2-3 minutes, and control the material discharge temperature of the internal mixer to be 105-110°C. After the mixing is completed, a cable sheath material with high wear resistance and high mechanical strength can be obtained.

[0026] By adopting the above technical scheme, the method of the present application sequentially feeds chlorosulfonated polyethylene, additives, vulcanizers and vulcanization accelerators, and obtains a cable sheath material with high wear resistance and high mechanical strength after mixing.

[0027] In summary, this application has the following beneficial effects: 1. This application uses chlorosulfonated polyethylene and wollastonite nanotubes to reinforce the chlorosulfonated polyethylene by using the pulling effect between wollastonite nanotubes and chlorosulfonated polyethylene, thereby improving the tear resistance of the cable sheath material. At the same time, the good hardness and rigidity of the wollastonite nanotubes themselves also improve the wear resistance of the cable sheath material. By using the cable sheath material of this application in cable production, it can fully adapt to the operating conditions of coal mines, reduce the damage to the cable caused by the combined effect of internal tension and ground resistance, and extend the service life of the cable. It has good application prospects in the mining cable industry.

[0028] 2. The preferred auxiliary agent in the present application also includes a surfactant, and the surfactant has a carbon-carbon double bond in its molecule. During the processing, the surfactant is adsorbed on the wollastonite nanotubes, and the carbon-carbon double bonds are crosslinked with the chlorosulfonated polyethylene by vulcanization, which not only increases the degree of crosslinking by vulcanization of the chlorosulfonated polyethylene, but also improves the bonding degree between the wollastonite nanotubes and the chlorosulfonated polyethylene, thereby improving the tear resistance and wear resistance of the cable sheath material. DETAILED DESCRIPTION

[0029] The present application is further described in detail below in conjunction with embodiments, preparation examples and comparative examples. The raw materials involved in the present application can all be obtained commercially.

[0030] In the following examples and comparative examples, the model of the chlorosulfonated polyethylene used is Tosoh TS-530, and the model of the chlorinated polyethylene used is CM352.

[0031] Preparation Example of Wollastonite Nanotubes Preparation Example 1-5 The following is an explanation using Preparation Example 1.

[0032] Preparation Example 1 In this preparation example, wollastonite nanotubes were prepared according to the following method: (1) Sodium silicate and calcium nitrate are added to water to prepare a 0.5 mol / L solution, and then polyethylene glycol is added to the calcium nitrate solution to make the mass fraction of polyethylene glycol in the calcium nitrate solution be 0.5%, and then the sodium silicate solution is added dropwise to the calcium nitrate solution, and stirring is continued during the dropping process, and the calcium nitrate solution is filtered after no more precipitation occurs, and the precipitate obtained by filtration is washed and dried to obtain a nanotube precursor; (2) A nanotube precursor, sodium nitrate, and anhydrous sodium carbonate are mixed in a weight ratio of 1:5:0.2 and ground to obtain a mixture; the mixture is heated at 350° C. for 2 h, and the mixture is washed after cooling until the pH of the washing liquid is 7, and the washing residue is dried to obtain wollastonite nanotubes.

[0033] As shown in Table 1, the difference between Preparation Examples 1-5 is that the nanotube precursor, sodium nitrate, and anhydrous sodium carbonate are mixed in different weight ratios (hereinafter referred to as weight ratio).

[0034] Table 1 Weight ratio of nanotube precursor, sodium nitrate and anhydrous sodium carbonate sample Preparation Example 1 Preparation Example 2 Preparation Example 3 Preparation Example 4 Preparation Example 5 Weight Ratio 1:5:0.2 1:5:0.3 1:5:0.35 1:5:0.4 1:5:0.5 Example

[0035] Examples 1-5 The following description is given by taking Example 1 as an example.

[0036] Example 1 In this embodiment, the vulcanizing agent is BIBP, the vulcanizing aid is TAIC, the plasticizer is chlorinated paraffin (CAS No.: 63449-39-8), the flame retardant is clay (CAS No.: 70131-50-9), the antioxidant is antioxidant RD (CAS No.: 26780-96-1), and the wollastonite nanotubes are commercially available wollastonite nanotubes, and the average diameter of the wollastonite nanotubes is 80 nm.

[0037] In this embodiment, the cable sheath material with high wear resistance and high mechanical strength is prepared according to the following steps: (1) 10 kg of zinc oxide, 15 kg of plasticizer, 5 kg of lead stearate, 3 kg of antioxidant, 20 kg of flame retardant, 30 kg of white carbon black, 10 kg of wollastonite nanotubes, and 10 kg of talc are mixed to obtain an auxiliary agent for standby use; (2) Add 100 kg of chlorosulfonated polyethylene into an internal mixer and heat it to 75° C. (3) Add the additives into an internal mixer and mix for 2 minutes; (4) 3 kg of vulcanizing agent and 2 kg of vulcanization accelerator are added to the internal mixer and kneaded for 2 minutes, and the material discharge temperature of the internal mixer is controlled to be 108° C. After the kneading is completed, a cable sheath material with high wear resistance and high mechanical strength can be obtained.

[0038] After obtaining the cable sheath material, continue to use the open mill to turn the material, and then use the three-roll calender to calender it into sheets, and then store it in a dry oven.

[0039] As shown in Table 2, the main difference between Examples 1-5 is that the raw material ratios of the cable sheath material are different.

[0040] Table 2 Raw material ratio of cable sheath material Example 6 The difference between this embodiment and embodiment 3 is that the auxiliary agent further comprises a surfactant, and the surfactant is oleyl alcohol polyoxyethylene ether (EO=2), and the amount of oleyl alcohol polyoxyethylene ether is 2.2% of the weight of the wollastonite nanotubes.

[0041] Example 7 The difference between this embodiment and embodiment 6 is that oleyl alcohol polyoxyethylene ether is replaced by sodium oleyl alcohol polyoxyethylene ether sulfonate (EO=2).

[0042] As shown in Table 3, the difference between Examples 7-11 is that the percentage of the amount of sodium oleyl alcohol polyoxyethylene ether sulfonate used in the weight of wollastonite nanotubes (hereinafter referred to as percentage R1) is different.

[0043] Table 3 R1 sample Example 7 Example 8 Example 9 Example 10 Embodiment 11 R1 / % 2.2 2.6 3.0 3.4 3.8 Example 12 The difference between this embodiment and embodiment 11 is that the wollastonite nanotubes are prepared according to the method of preparation example 1.

[0044] As shown in Table 4, the difference between Examples 12-16 is that the preparation examples of wollastonite nanotubes are different.

[0045] Table 4 Preparation example of wollastonite nanotubes sample Example 12 Embodiment 13 Embodiment 14 Embodiment 15 Example 16 Preparation Example Preparation Example 1 Preparation Example 2 Preparation Example 3 Preparation Example 4 Preparation Example 5 Examples 17-20 As shown in Table 5, the difference between Examples 17-20 and Example 16 is that the percentage of the amount of sodium oleyl alcohol polyoxyethylene ether sulfonate used in the weight of wollastonite nanotubes (hereinafter referred to as percentage R2) is different.

[0046] Table 5 R2 Embodiment 21 The difference between this embodiment and embodiment 19 is that the surfactant further comprises oleyl alcohol polyoxyethylene ether, and the amount of oleyl alcohol polyoxyethylene ether used is 25% of the weight of oleyl alcohol polyoxyethylene ether sodium sulfonate.

[0047] As shown in Table 6, the difference between Examples 21-25 is that the percentage of the amount of oleyl alcohol polyoxyethylene ether to the weight of sodium oleyl alcohol polyoxyethylene ether sulfonate (hereinafter referred to as percentage R3) is different.

[0048] Table 6 R3 Comparative Example Comparative Example 1 The difference between this comparative example and Example 3 is that the chlorosulfonated polyethylene is replaced by chlorinated polyethylene, and the components of the auxiliary agent do not include wollastonite nanotubes.

[0049] Comparative Example 2 The difference between this comparative example and Example 3 is that the auxiliary agent does not include wollastonite nanotubes.

[0050] Comparative Example 3 This comparative example is different from Example 3 in that the mass of chlorosulfonated polyethylene is replaced by chlorinated polyethylene.

[0051] Performance testing methods 1. Tear strength The tear strength of the cable sheath material was tested with reference to “JB / T 10696.7-2007 Test methods for mechanical and physical and chemical properties of wires and cables Part 7: Tear test”. The results are shown in Table 7.

[0052] Table 7 Tear strength 2. Comprehensive performance The cable sheath materials of Example 3 and Comparative Example 1 were subjected to comprehensive performance tests, and the results are shown in Table 8.

[0053] Table 8 Comprehensive performance test Combining Examples 1-5 and Comparative Example 1 and Table 7, it can be seen that the tear strength measured in Examples 1-5 is greater than that in Comparative Example 1, indicating that the present application, through the coordination between chlorosulfonated polyethylene and wollastonite nanotubes, electrostatic adsorption occurs between calcium ions in calcium metasilicate and sulfonic acid groups in chlorosulfonated polyethylene, which has a pulling effect on the molecules of chlorosulfonated polyethylene, thereby improving the tear resistance of the cable sheath material. By using the cable sheath material of the present application in cable production, it can fully adapt to the harsh operating conditions of coal mines, reduce the damage to the cable caused by the combined action of internal tension and ground resistance, and thus extend the service life of the cable, and has good application prospects in the mining cable industry.

[0054] Combining Example 3 and Comparative Examples 2-3 and Table 7, it can be seen that when wollastonite nanotubes are not used in combination with chlorosulfonated polyethylene, the two cannot produce a pulling effect through electrostatic adsorption, so the tear resistance of the cable sheath material is poor.

[0055] Combining Example 3 and Examples 6-7 with Table 7, it can be seen that sodium oleyl alcohol polyoxyethylene ether sulfonate can be more fully adsorbed to wollastonite nanotubes than oleyl alcohol polyoxyethylene ether, indicating that electrostatic adsorption makes the adsorption effect between the anionic surfactant and the wollastonite nanotubes better.

[0056] From Examples 7-11 and Table 7, it can be seen that increasing the amount of sodium oleyl alcohol polyoxyethylene ether sulfonate has a certain improvement effect on the tear strength, but as the amount of sodium oleyl alcohol polyoxyethylene ether sulfonate increases, the growth rate of the tear strength decreases, indicating that the adsorption of sodium oleyl alcohol polyoxyethylene ether sulfonate by wollastonite nanotubes is gradually approaching saturation, and it is difficult to further adsorb more sodium oleyl alcohol polyoxyethylene ether sulfonate.

[0057] Combining Example 11, Examples 12-16 and Table 7, it can be seen that the tear strength of Examples 12-16 first shows an upward trend, and then tends to be flat after Example 14. Among them, the tear strength measured in Example 12 is relatively small, indicating that the calcium ion distribution density on the surface of the wollastonite nanotubes of Preparation Example 1 is relatively low. The tear strength of Examples 15 and 16 does not change much compared with Example 14, indicating that in Example 14, sodium oleyl alcohol polyoxyethylene ether sulfonate has been almost completely adsorbed. Therefore, considering the production cost and actual effect, when the amount of sodium oleyl alcohol polyoxyethylene ether sulfonate is 3.8% of the weight of the wollastonite nanotubes, the wollastonite nanotubes of Preparation Example 3 can fully adsorb sodium oleyl alcohol polyoxyethylene ether sulfonate.

[0058] It can be seen from Example 16, Examples 17-20 and Table 7 that, when the amount of sodium oleyl alcohol polyoxyethylene ether sulfonate molecules is further increased on the basis of Example 16, sodium oleyl alcohol polyoxyethylene ether sulfonate will continue to be adsorbed by the wollastonite nanotubes, thereby further increasing the bonding degree between the wollastonite nanotubes and the chlorosulfonated polyethylene, and improving the tear resistance of the cable sheath material. However, due to the electrostatic repulsion between the sodium oleyl alcohol polyoxyethylene ether sulfonate molecules, the adsorption amount of the sodium oleyl alcohol polyoxyethylene ether sulfonate gradually tends to saturation during the increase in the amount of sodium oleyl alcohol polyoxyethylene ether sulfonate, which limits the growth of the tear strength.

[0059] It can be seen from Example 19, Examples 21-25 and Table 7 that oleyl alcohol polyoxyethylene ether can be inserted between adjacent oleyl alcohol polyoxyethylene ether sodium sulfonates, reducing the repulsion between sulfonic acid groups, and further increasing the distribution density of the surfactant on the surface of wollastonite nanotubes when the adsorption of oleyl alcohol polyoxyethylene ether sodium sulfonate reaches saturation, thereby increasing the bonding degree between wollastonite nanotubes and chlorosulfonated polyethylene and improving the tear resistance of the cable sheath material.

[0060] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A cable sheath material with high wear resistance and high mechanical strength, characterized in that: The cable sheath material is obtained by mixing an auxiliary agent, 100 parts by weight of chlorosulfonated polyethylene, 3-5 parts by weight of a vulcanizing agent, and 2-3.5 parts by weight of a vulcanization accelerator. The auxiliary agent includes the following components in parts by weight: 10-15 parts of zinc oxide, 15-30 parts of a plasticizer, 5-10 parts of lead stearate, 3-5 parts of an antioxidant, 20-30 parts of a flame retardant, 30-50 parts of white carbon black, 10-15 parts of wollastonite nanotubes, and 10-15 parts of talc.

2. The cable sheath material with high wear resistance and high mechanical strength according to claim 1, characterized in that: The components of the auxiliary agent also include a surfactant, and the surfactant has a carbon-carbon double bond in its molecule.

3. The cable sheath material with high wear resistance and high mechanical strength according to claim 2, characterized in that: The surfactant includes sodium oleyl alcohol polyoxyethylene ether sulfonate.

4. The cable sheath material with high wear resistance and high mechanical strength according to claim 3, characterized in that: The dosage of the sodium oleyl alcohol polyoxyethylene ether sulfonate is 2.6-3.4% of the weight of the wollastonite nanotubes.

5. The cable sheath material with high wear resistance and high mechanical strength according to claim 3, characterized in that: The wollastonite nanotubes are prepared according to the following method: (1) Sodium silicate and calcium nitrate are added to water to prepare a solution, polyethylene glycol is added to the calcium nitrate solution, and then the sodium silicate solution is added dropwise to the calcium nitrate solution, and stirring is continued during the dropping process. After no more precipitation appears in the calcium nitrate solution, the solution is filtered, and the precipitate obtained by filtration is washed and dried to obtain a nanotube precursor; (2) A nanotube precursor, sodium nitrate, and anhydrous sodium carbonate are mixed in a weight ratio of 1:5:(0.3-0.5) and ground to obtain a mixture; the mixture is heated at 350° C. for 2 h, and after cooling, the mixture is washed until the pH of the washing solution is 7, and the washing residue is dried to obtain wollastonite nanotubes.

6. The cable sheath material with high wear resistance and high mechanical strength according to claim 5, characterized in that: The nanotube precursor, sodium nitrate and anhydrous sodium carbonate are mixed in a weight ratio of 1:5:0.35, and the amount of sodium oleyl alcohol polyoxyethylene ether sulfonate used is 3.8% of the weight of the wollastonite nanotubes.

7. The cable sheath material with high wear resistance and high mechanical strength according to claim 5, characterized in that: The nanotube precursor, sodium nitrate and anhydrous sodium carbonate are mixed in a weight ratio of 1:5:0.5, and the amount of sodium oleyl alcohol polyoxyethylene ether sulfonate is 4.2-6.0% of the weight of the wollastonite nanotubes.

8. The cable sheath material with high wear resistance and high mechanical strength according to claim 7, characterized in that: The dosage of the sodium oleyl alcohol polyoxyethylene ether sulfonate is 6.0% of the weight of the wollastonite nanotubes, and the surfactant also includes oleyl alcohol polyoxyethylene ether.

9. The cable sheath material with high wear resistance and high mechanical strength according to claim 8, characterized in that: The amount of the oleyl alcohol polyoxyethylene ether used is 28-36% of the weight of the sodium oleyl alcohol polyoxyethylene ether sulfonate.

10. A method for preparing a cable sheath material with high wear resistance and high mechanical strength, characterized in that: The following steps are involved: (1) Prepare the auxiliary agent according to any one of claims 1 to 9 and set it aside; (2) Add chlorosulfonated polyethylene into an internal mixer and heat it to 70-80°C; (3) Add the additives into an internal mixer and mix for 2-3 minutes; (4) Add the vulcanizing agent and the vulcanization accelerator into the internal mixer and continue mixing for 2-3 minutes. Control the material discharge temperature of the internal mixer to be 105-110°C. After mixing, a cable sheath material with high wear resistance and high mechanical strength can be obtained.

Citation Information

Patent Citations

  • Mine-cable rubber sheathing material and preparation process

    CN102924834A

  • High strength high tearing strength extra heavy load jacket rubber and preparation method thereof

    CN103205063A

  • High-tear-resistance high-wear-resistance chlorinated polyethylene cable sheath material for mining cables and preparation method thereof

    CN111286129A

  • Rubber composite material for cables as well as preparation method and application of rubber composite material

    CN113045834A

  • Wire / cable and composition

    JP2013041794A