Electromagnetic shielding heat shrink tube and preparation method thereof

By chemically modifying carbon nanotubes and grafting them onto the heat shrink tube through irradiation cross-linking technology, the problem of poor electromagnetic shielding performance of the heat shrink tube is solved, and a heat shrink tube with excellent electromagnetic shielding performance and multiple advantages is prepared. Suitable for reducing electromagnetic interference and improving equipment safety.

CN118895029APending Publication Date: 2024-11-05SHANGHAI CHANGYUAN ELECTRONICS MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310492943.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-05
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing heat shrink tubes lack electromagnetic shielding performance, resulting in serious electromagnetic wave interference problems, affecting the normal operation of electronic equipment and information security.

Method used

By chemically modifying the carbon nanotubes and grafting them onto the heat-shrinking tube matrix material by irradiation and crosslinking, a heat-shrinking tube with electromagnetic shielding function is prepared, including the inner glue layer and the outer skin layer. The outer skin layer consists of modified carbon nanotubes, fluoroelastomer, vinylidene fluoride resin, carbon black and filler.

Benefits of technology

The prepared electromagnetic shielding heat shrink tube has excellent electromagnetic shielding performance, conductivity, insulation performance and wear resistance, which can effectively reduce electromagnetic interference and is suitable for large-scale mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895029A_ABST
    Figure CN118895029A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an electromagnetic shielding heat-shrinkable tube, which comprises the following steps: chemically modifying a carbon nano tube, and grafting the carbon nano tube on a heat-shrinkable tube base material in an irradiation crosslinking manner to prepare the heat-shrinkable tube with an electromagnetic shielding function. In the modified carbon nanotubes, carbon atoms contain unbonded electrons and can directionally move under the action of external current, so that the modified carbon nanotubes have an excellent electrostatic shielding function. Through irradiation crosslinking of an electron accelerator, the modified carbon nanotubes are covalently bonded on a polymer matrix material, so that the filling firmness of the carbon nanotubes in the polymer material is improved. The invention further provides an electromagnetic shielding heat shrink tube, the heat shrink tube comprises an inner rubber layer and an outer skin layer with electromagnetic shielding performance, and the outer skin layer is composed of the modified carbon nano tube, fluororubber, carbon black and filler. The heat-shrinkable tube provided by the invention has excellent electromagnetic shielding performance, the preparation process is simple, and the raw materials are wide in source.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of heat shrink tubes, and further relates to an electromagnetic shielding heat shrink tube and a preparation method thereof. Background Art

[0002] Electromagnetic waves are a major way of electromagnetic energy propagation. When a circuit is working, it will radiate electromagnetic waves, which will cause electromagnetic interference to other nearby devices. On the other hand, various electromagnetic waves in space will also be induced into the circuit and cause interference to the circuit.

[0003] In order to reduce the interference of electromagnetic waves, people are committed to electromagnetic shielding. Electromagnetic shielding is the simplest and most effective method to eliminate interference by cutting off the propagation path of electromagnetic waves. It is mainly used in military and national defense, aerospace, electronic communications, petrochemicals, instrumentation, medical and other fields.

[0004] Heat shrink tubing is widely used in cable assembly, but ordinary heat shrink tubing usually does not have electromagnetic shielding performance. The electromagnetic interference problem caused by electromagnetic waves is becoming increasingly serious, not only causing interference and damage to electronic instruments and equipment, but also easily causing information leakage. Summary of the invention

[0005] In view of the problem that the electromagnetic shielding performance of heat shrinkable tubes in the prior art is poor, the purpose of the present invention is to provide an electromagnetic shielding heat shrinkable tube and a preparation method thereof. The present invention chemically modifies carbon nanotubes and grafts them onto the heat shrinkable tube base material by radiation cross-linking to prepare an electromagnetic shielding heat shrinkable tube with excellent electromagnetic shielding function.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for preparing an electromagnetic shielding heat shrinkable tube, characterized in that carbon nanotubes are chemically treated and modified, and are grafted onto a heat shrinkable tube base material by radiation cross-linking to prepare a heat shrinkable tube with electromagnetic shielding function.

[0008] In some technical solutions, the chemical treatment and modification of carbon nanotubes comprises the following steps:

[0009] S1, placing hydroxylated carbon nanotubes, an acid binding agent and a solvent in a container and subjecting them to magnetic stirring to obtain a mixture; S2, adding an enoyl chloride reagent to the mixture and continuing the reaction; S3, washing and filtering the mixture after the reaction to obtain modified carbon nanotubes.

[0010] In some technical schemes, the acid binding agent is one or a mixture of two or more of triethylamine, pyridine and NN diisopropylethylamine; and / or, the solvent is one or a mixture of two of chloroform and dichloromethane; and / or, the solvent needs to be freshly distilled to remove water.

[0011] In some technical solutions, the enoyl chloride reagent is one or a mixture of two or more of acryloyl chloride, methacryloyl chloride, crotonoyl chloride and 10-undecenoyl chloride; and / or the enoyl chloride reagent needs to be added dropwise to the mixture.

[0012] In some technical solutions, in step S1: the magnetic stirring time is 30 minutes; and / or, the reaction temperature for continuing the reaction after adding the enamine reagent to the mixture is 20-50° C., and the reaction time is 2-48 hours.

[0013] In some technical solutions, the radiation dose required for the radiation cross-linking is 50 to 250 kGy.

[0014] The present invention also discloses an electromagnetic shielding heat shrink tube, comprising an inner rubber layer and an outer skin layer with electromagnetic shielding properties, wherein the components of the inner rubber layer include fluororubber, vinylidene fluoride resin and filler; the components of the outer skin layer include modified carbon nanotubes and fluororubber, vinylidene fluoride resin, carbon black and filler.

[0015] In some technical schemes, the inner rubber layer includes the following components in mass proportions: 50 to 100 parts of fluororubber, 5 to 30 parts of vinyl fluoride resin, and 1 to 30 parts of filler; the outer skin layer includes the following components in mass proportions: 1 to 30 parts of modified carbon nanotubes, 50 to 100 parts of fluororubber, 10 to 50 parts of vinyl fluoride resin, 3 to 30 parts of carbon black, and 1 to 30 parts of filler.

[0016] In some technical solutions, the vinylidene fluoride resin is a mixture of one or both of homopolyvinylidene fluoride and copolymerized vinylidene fluoride; and / or, the Mooney viscosity of the fluororubber used in the inner rubber layer is 10 to 30 (Mn121℃1+10).

[0017] In some technical schemes, the preparation method of an electromagnetic shielding heat shrink tube comprises the following steps: S4, respectively weighing and mixing the components of the inner rubber layer and the outer skin layer according to the mass ratio, and obtaining the inner rubber material and the outer skin material through mixing and granulation; S5, extruding the inner rubber material and the outer skin material into a double-wall hollow tube through two combined single-screw extruders equipped with a double-wall heat shrink tube co-extrusion mold; S6, irradiating and cross-linking the double-wall hollow tube through an electron accelerator, heating and expanding it in a glycerin oil tank, and cooling and shaping to obtain a finished double-wall heat shrink tube with electromagnetic shielding properties.

[0018] Compared with the prior art, the present invention can bring the following beneficial effects:

[0019] 1. The present invention provides a method for preparing an electromagnetic shielding heat shrinkable tube, wherein the carbon nanotubes are chemically modified and grafted onto a heat shrinkable tube substrate by radiation cross-linking. The carbon atoms in the carbon nanotubes contain unbonded electrons, which can move in a directional manner under the action of an external current. The heat shrinkable tube prepared has an excellent electrostatic shielding function.

[0020] 2. The carbon nanotubes provided by the present invention are modified by chemical treatment to contain double bonds. After being irradiated by an electron accelerator, they can be chemically bonded with the polymer material matrix, thereby ensuring the dispersibility and filling firmness of the carbon nanotubes in the polymer material. The electromagnetic shielding heat shrinkable tube prepared has the advantage of maintaining good electrical conductivity for a long time.

[0021] 3. The present invention also provides an electromagnetic shielding heat shrinkable tube, which comprises an inner rubber layer and an outer skin layer with electromagnetic shielding properties, wherein the outer skin layer is composed of modified carbon nanotubes, fluororubber, vinylidene fluoride resin, carbon black and filler. The heat shrinkable tube not only has excellent electromagnetic shielding performance and conductive performance, but also has the advantages of good insulation performance and wear resistance.

[0022] 4. The heat shrinkable tube provided by the present invention is simple to prepare, has a wide range of raw material sources, good compatibility between raw materials, strong plasticity, convenient transportation and installation, and is suitable for large-scale mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0024] Figure 1 A synthetic route map of the modified carbon nanotubes provided by the present invention;

[0025] Figure 2 This is a schematic diagram of the structure of the modified carbon nanotubes and the outer skin resin matrix cross-linked provided by the present invention. DETAILED DESCRIPTION

[0026] The present invention is further described below in conjunction with specific embodiments, but these embodiments are only exemplary and do not constitute any limitation on the scope of the present invention. It should be understood by those skilled in the art that several improvements and modifications may be made without departing from the principles of the present invention, and these improvements and modifications should also be considered as the protection scope of the present invention.

[0027] Example 1

[0028] The present invention provides a method for preparing an electromagnetic shielding heat shrink tube, wherein carbon nanotubes are chemically treated and modified, and then grafted onto a heat shrink tube substrate material by radiation cross-linking to prepare a heat shrink tube with electromagnetic shielding function.

[0029] In this embodiment, chemical treatment and modification of carbon nanotubes includes the following steps:

[0030] S1, placing hydroxylated carbon nanotubes, an acid binding agent, and a solvent in a container and subjecting them to magnetic stirring for 30 minutes to obtain a mixture;

[0031] S2, after adding enoyl chloride reagent dropwise into the mixture, continue the reaction at 20-50° C. for 2-48 hours;

[0032] S3, washing and filtering the mixture after the reaction to obtain modified carbon nanotubes.

[0033] like Figure 1 and Figure 2 As shown, the carbon nanotubes are modified by chemical treatment. The modified carbon nanotubes contain double bonds. They are grafted onto the heat shrink tube matrix material by radiation cross-linking and chemically bonded to the polymer matrix, ensuring the dispersion and filling firmness of the carbon nanotubes in the polymer material, so that it maintains good conductivity for a long time. The carbon atoms in the carbon nanotubes contain unbonded electrons, which can move in a directional manner under the action of external current. Therefore, the heat shrink tube made of carbon nanotubes exhibits electrostatic shielding function.

[0034] Preferably, the acid binding agent is one or a mixture of two or more of triethylamine, pyridine and NN diisopropylethylamine; the solvent is one or a mixture of two of chloroform and dichloromethane; and the solvent needs to be freshly distilled to remove water.

[0035] Preferably, the enoyl chloride reagent is one or a mixture of two or more of acryloyl chloride, methacryloyl chloride, crotonoyl chloride and 10-undecenoyl chloride.

[0036] Preferably, the radiation dose required for radiation cross-linking is 50 to 250 kGy.

[0037] Example 2

[0038] The present invention also proposes an electromagnetic shielding heat shrinkable tube and a preparation method thereof. The heat shrinkable tube comprises an inner rubber layer and an outer skin layer with electromagnetic shielding properties, wherein the inner rubber layer comprises the following components in parts by mass: 50 to 100 parts of fluororubber, 5 to 30 parts of vinyl fluoride resin, and 1 to 30 parts of filler; the outer skin layer comprises the following components in parts by mass: 1 to 30 parts of modified carbon nanotubes, 50 to 100 parts of fluororubber, 10 to 50 parts of vinyl fluoride resin, 3 to 30 parts of carbon black, and 1 to 30 parts of filler.

[0039] Preferably, the vinylidene fluoride resin is one or a mixture of homopolyvinylidene fluoride and copolymerized vinylidene fluoride.

[0040] Preferably, the Mooney viscosity of the fluororubber used in the inner rubber layer is 10 to 30 (Mn121°C 1+10).

[0041] Based on the steps of Example 1, the preparation steps of the electromagnetic shielding heat shrink tube further include:

[0042] S4, respectively weighing and mixing the components of the inner rubber layer and the outer skin layer according to the mass ratio, and obtaining the inner rubber material and the outer skin material by mixing and granulating;

[0043] S5, extruding the inner rubber material and the outer skin material into a double-wall hollow tube through two combined single screws equipped with a double-wall heat shrink tube co-extrusion die;

[0044] S6. The double-wall hollow tube is irradiated and cross-linked by an electron accelerator, heated and expanded in a glycerin oil tank, and cooled and shaped to obtain a double-wall heat shrink tube with electromagnetic shielding properties.

[0045] In order to better understand and apply the above scheme and effectively demonstrate the corresponding benefits, the present application also provides a variety of embodiments as described below.

[0046] Example 3

[0047] S1, taking 100 g of hydroxylated carbon nanotubes and 0.1 mol of an acid binding agent, pouring into 450 ml of a solvent, placing in a flask and magnetically stirring for 30 min to obtain a mixture;

[0048] S2, add 0.1 mol of acryloyl chloride reagent to the mixture, react at 40°C for 12 hours;

[0049] S3, washing and filtering the mixture after the reaction to obtain modified carbon nanotubes;

[0050] S4, according to the mass fraction,

[0051] The inner rubber layer is made of 100 parts of fluororubber, 30 parts of vinylidene fluoride resin, and 10 parts of filler.

[0052] The outer layer preparation components are: 5 parts of modified carbon nanotubes, 100 parts of fluororubber, 30 parts of vinylidene fluoride resin, 5 parts of carbon black, and 10 parts of filler.

[0053] The inner rubber layer raw material and the outer skin layer raw material are mixed and granulated to obtain the inner rubber material and the outer skin material respectively;

[0054] S5, extruding the inner rubber material and the outer skin material into a double-wall hollow tube through two combined single screws equipped with a double-wall heat shrink tube co-extrusion die;

[0055] S6. The double-walled hollow tube is irradiated and cross-linked by an electron accelerator with an irradiation dose of 170 kGy, heated and expanded in a glycerol oil tank, and cooled and shaped to obtain a heat shrink tube with electromagnetic shielding properties. The electromagnetic shielding effectiveness of the prepared tube is ≥10 dB.

[0056] Example 4

[0057] S1, taking 100 g of hydroxylated carbon nanotubes and 0.2 mol of an acid binding agent, pouring into 450 ml of a solvent, placing in a flask and magnetically stirring for 30 min to obtain a mixture;

[0058] S2, add 0.2 mol of acryloyl chloride reagent to the mixture, react at 40°C for 12 hours;

[0059] S3, washing and filtering the mixture after the reaction to obtain modified carbon nanotubes;

[0060] S4, according to the mass fraction,

[0061] The inner rubber layer is made of 100 parts of fluororubber, 30 parts of vinylidene fluoride resin, and 10 parts of filler.

[0062] The outer layer preparation components are: 5 parts of modified carbon nanotubes, 100 parts of fluororubber, 30 parts of vinylidene fluoride resin, 5 parts of carbon black, and 10 parts of filler.

[0063] The inner rubber layer raw material and the outer skin layer raw material are mixed and granulated to obtain the inner rubber material and the outer skin material respectively;

[0064] S5, extruding the inner rubber material and the outer skin material into a double-wall hollow tube through two combined single screws equipped with a double-wall heat shrink tube co-extrusion die;

[0065] S6. The double-walled hollow tube is irradiated and cross-linked by an electron accelerator with an irradiation dose of 170 kGy, heated and expanded in a glycerol oil tank, and cooled and shaped to obtain a heat shrink tube with electromagnetic shielding properties. The electromagnetic shielding effectiveness of the prepared tube is ≥10 dB.

[0066] Example 5

[0067] S1, taking 100 g of hydroxylated carbon nanotubes and 0.2 mol of an acid binding agent, pouring into 450 ml of a solvent, placing in a flask and magnetically stirring for 30 min to obtain a mixture;

[0068] S2, add 0.2 mol of methacryloyl chloride reagent to the mixture, react at 40°C for 12 hours;

[0069] S3, washing and filtering the mixture after the reaction to obtain modified carbon nanotubes;

[0070] S4, according to the mass fraction,

[0071] The inner rubber layer is made of 100 parts of fluororubber, 30 parts of vinylidene fluoride resin, and 10 parts of filler.

[0072] The outer layer preparation components are: 10 parts of modified carbon nanotubes, 100 parts of fluororubber, 30 parts of vinylidene fluoride resin, 5 parts of carbon black, and 10 parts of filler.

[0073] The inner rubber layer raw material and the outer skin layer raw material are mixed and granulated to obtain the inner rubber material and the outer skin material respectively;

[0074] S5, extruding the inner rubber material and the outer skin material into a double-wall hollow tube through two combined single screws equipped with a double-wall heat shrink tube co-extrusion die;

[0075] S6. The double-walled hollow tube is irradiated and cross-linked by an electron accelerator with an irradiation dose of 170 kGy, heated and expanded in a glycerol oil tank, and cooled and shaped to obtain a heat shrink tube with electromagnetic shielding properties. The electromagnetic shielding effectiveness of the prepared tube is ≥20 dB.

[0076] Example 6

[0077] S1, taking 100 g of hydroxylated carbon nanotubes and 0.2 mol of an acid binding agent, pouring into 450 ml of a solvent, placing in a flask and magnetically stirring for 30 min to obtain a mixture;

[0078] S2, add 0.2 mol of methacryloyl chloride reagent to the mixture, react at 40°C for 12 hours;

[0079] S3, washing and filtering the mixture after the reaction to obtain modified carbon nanotubes;

[0080] S4, according to the mass fraction,

[0081] The inner rubber layer is made of 100 parts of fluororubber, 30 parts of vinylidene fluoride resin, and 10 parts of filler.

[0082] The outer layer preparation components are: 20 parts of modified carbon nanotubes, 100 parts of fluororubber, 30 parts of vinylidene fluoride resin, 5 parts of carbon black, and 10 parts of filler.

[0083] The inner rubber layer raw material and the outer skin layer raw material are mixed and granulated to obtain the inner rubber material and the outer skin material respectively;

[0084] S5, extruding the inner rubber material and the outer skin material into a double-wall hollow tube through two combined single screws equipped with a double-wall heat shrink tube co-extrusion die;

[0085] S6. Double-walled hollow tubes are cross-linked by irradiation with an electron accelerator, with an irradiation dose of 170 kGy, heated and expanded in a glycerol tank, and cooled and shaped to obtain a heat shrink tube with electromagnetic shielding properties. The electromagnetic shielding effectiveness of the prepared tube is ≥40 dB.

[0086] Example 7

[0087] S1, taking 100 g of hydroxylated carbon nanotubes and 0.2 mol of an acid binding agent, pouring into 450 ml of a solvent, placing in a flask and magnetically stirring for 30 min to obtain a mixture;

[0088] S2, add 0.2 mol of methacryloyl chloride reagent to the mixture, react at 40°C for 12 hours;

[0089] S3, washing and filtering the mixture after the reaction to obtain modified carbon nanotubes;

[0090] S4, according to the mass fraction,

[0091] The inner rubber layer is made of 100 parts of fluororubber, 30 parts of vinylidene fluoride resin, and 10 parts of filler.

[0092] The outer layer preparation components are: 40 parts of modified carbon nanotubes, 100 parts of fluororubber, 30 parts of vinylidene fluoride resin, 5 parts of carbon black, and 10 parts of filler.

[0093] The inner rubber layer raw material and the outer skin layer raw material are mixed and granulated to obtain the inner rubber material and the outer skin material respectively;

[0094] S5, extruding the inner rubber material and the outer skin material into a double-wall hollow tube through two combined single screws equipped with a double-wall heat shrink tube co-extrusion die;

[0095] S6. Double-walled hollow tubes are cross-linked by irradiation with an electron accelerator, with an irradiation dose of 170 kGy, heated and expanded in a glycerol oil tank, and cooled and shaped to obtain a heat shrink tube with electromagnetic shielding properties. The electromagnetic shielding effectiveness of the prepared tube is ≥ 60 dB.

[0096] The above are only preferred embodiments of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing an electromagnetic shielding heat shrinkable tube, characterized in that: The carbon nanotubes are modified by chemical treatment and grafted onto a heat shrink tube matrix material by radiation cross-linking to prepare a heat shrink tube with electromagnetic shielding function.

2. The method for preparing the electromagnetic shielding heat shrinkable tube according to claim 1, characterized in that: The chemical treatment and modification of carbon nanotubes comprises the following steps: S1, placing hydroxylated carbon nanotubes, an acid binding agent, and a solvent in a container and performing magnetic stirring to obtain a mixture; S2, adding an enoyl chloride reagent to the mixture and continuing the reaction; S3, washing and filtering the mixture after the reaction to obtain modified carbon nanotubes.

3. The method for preparing the electromagnetic shielding heat shrinkable tube according to claim 2, characterized in that: The acid binding agent is one or a mixture of two or more of triethylamine, pyridine and NN diisopropylethylamine; and / or, The solvent is chloroform and dichloromethane or a mixture of both; and / or, The solvent needs to be freshly distilled to remove water.

4. The method for preparing the electromagnetic shielding heat shrinkable tube according to claim 2, characterized in that: The enoyl chloride reagent is one or a mixture of two or more of acryloyl chloride, methacryloyl chloride, crotonoyl chloride and 10-undecenoyl chloride; and / or, The enoyl chloride reagent needs to be added dropwise into the mixture.

5. The method for preparing the electromagnetic shielding heat shrinkable tube according to claim 2, characterized in that: In step S1: The magnetic stirring time is 30 min; and / or, The reaction temperature for continuing the reaction after adding the enoyl chloride reagent to the mixture is 20 to 50° C. and the reaction time is 2 to 48 hours.

6. The method for preparing the electromagnetic shielding heat shrinkable tube according to claim 1, characterized in that: The radiation dose required for the radiation cross-linking is 50 to 250 kGy.

7. An electromagnetic shielding heat shrink tube, characterized in that: It includes an inner rubber layer and an outer skin layer with electromagnetic shielding properties. The components of the inner rubber layer include fluororubber, vinylidene fluoride resin and filler; The components of the outer skin layer include the modified carbon nanotubes as described in any one of claims 1 to 6, as well as fluororubber, vinylidene fluoride resin, carbon black and filler.

8. The electromagnetic shielding heat shrinkable tube according to claim 7, characterized in that: The inner rubber layer comprises the following components in parts by weight: 50-100 parts of fluororubber, 5-30 parts of vinylidene fluoride resin, 1-30 parts of filler; The outer layer comprises the following components in parts by weight: 1 to 30 parts of modified carbon nanotubes, 50 to 100 parts of fluororubber, 10 to 50 parts of vinylidene fluoride resin, 3 to 30 parts of carbon black, and 1 to 30 parts of filler.

9. The electromagnetic shielding heat shrinkable tube according to claim 7, characterized in that: The vinylidene fluoride resin is one or a mixture of homopolyvinylidene fluoride and copolymerized vinylidene fluoride; and / or, The Mooney viscosity of the fluororubber used in the inner rubber layer is 10-30 (Mn121℃1+10).

10. A method for preparing an electromagnetic shielding heat shrinkable tube according to any one of claims 7 to 9, characterized in that: The steps include: S4, respectively weighing and mixing the components of the inner rubber layer and the outer skin layer according to the mass ratio, and obtaining the inner rubber material and the outer skin material by mixing and granulating; S5, extruding the inner rubber material and the outer skin material into a double-wall hollow tube through two combined single screws equipped with a double-wall heat shrink tube co-extrusion die; S6. The double-wall hollow tube is irradiated and cross-linked by an electron accelerator, heated and expanded in a glycerin oil tank, and cooled and shaped to obtain a double-wall heat shrink tube with electromagnetic shielding properties.