Novel organic-inorganic composite fluorescent silicon dioxide nano-microsphere and preparation method thereof

Naphthimide dye was modified by solvothermal method and covalently fixed on the surface of nano-silicon dioxide to prepare organic and inorganic composite fluorescent silica nano-microspheres with uniform particle size and high fluorescence efficiency, and solved the fluorescent microspheres in the prior art The complex spherical preparation and the lack of fluorescence function of nanosilicon dioxide have achieved widespread application in multiple fields.

CN118895119APending Publication Date: 2024-11-05HARBIN UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410938246.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing fluorescent microsphere preparation process is complex, has weak fluorescence, is prone to agglomeration and background fluorescence limitation, resulting in limited application fields, and the nanosilicon dioxide microspheres lack fluorescence function, limiting their wide range in catalysis, biology and medicine. application.

Method used

The naphthalimide dye is modified by solvothermal method to generate a silane coupling agent with high fluorescence function and hydrolysis function of silane coupling agent. The particle diameter is prepared by covalently fixing the fluorescence coupling agent on the surface of nano-silica. Organic and inorganic composite fluorescent silica nanometer microspheres with uniform and high fluorescence efficiency.

Benefits of technology

It realizes effective control of particle size uniformity and fluorescence intensity of fluorescent microspheres, reduces preparation costs, improves chemical stability and dispersion, and is suitable for light emitting devices, ion detection and microscopic detection of composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895119A_ABST
    Figure CN118895119A_ABST
Patent Text Reader

Abstract

The invention relates to a novel organic-inorganic composite fluorescent silicon dioxide nano-microsphere material and a preparation method thereof, and belongs to the technical field of material synthesis and detection. The method comprises the following steps: reacting a 1, 8-naphthalimide fluorescent monomer with a certain proportion of an isocyanate silane coupling agent to obtain an NAP-silane precursor which has a fluorescent function and a hydrolytic bonding function; and uniformly mixing the silanized fluorescent monomer and the nano silicon dioxide microspheres activated at high temperature in water and an ethanol solution according to a certain ratio, and reacting to obtain the yellow fluorescent silicon dioxide nano microspheres. The preparation method has the advantages that the process is simple, the cost is low, a complicated separation and purification process is not needed in the preparation process, and the prepared fluorescent nano-microspheres are uniform in size, high in fluorescence property and stable in chemical property and have potential application value in the fields of photoelectric materials, fluorescence labeling and medicine.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a nano silicon-based composite material, in particular to a method for preparing an organic-inorganic composite fluorescent silicon dioxide nano-microsphere, and is applied to the technical field of nano composite materials. Background Art

[0002] As a special functional microsphere, fluorescent microspheres are increasingly favored by scientific researchers for their stable morphological structure and stable and efficient luminous efficiency. The newly developed fluorescent microspheres have uniform particle size, good monodispersity, good stability and high luminous efficiency. Fluorescent microspheres generally refer to microspheres whose surface is marked with fluorescent substances (including surface coating) or whose internal structure contains fluorescent substances (such as embedding or polymerization), which can be stimulated to fluoresce when stimulated by external energy. It is a functional microsphere carrying fluorescent molecules, and its appearance can be any shape, generally spherical. The carrier of fluorescent microspheres can be a polymer or an inorganic material. According to the difference between the carrier and the fluorescent substance, it is generally divided into two categories: inorganic / organic fluorescent microspheres and organic / organic fluorescent microspheres. In recent years, with the in-depth research on fluorescent probe technology, people have been able to prepare a variety of fluorescent microspheres with particle sizes ranging from nanometers to submicrometers. Fluorescent microspheres have a relatively stable morphological structure and luminescent behavior, and are much less affected by external conditions such as solvents, heat, electricity, and magnetism than pure fluorescent compounds. However, due to their complex preparation process, weak fluorescence, easy aggregation, and background fluorescence, the application of fluorescent microspheres is strictly limited. Therefore, it is particularly important to overcome these problems through reasonable structural design and process design.

[0003] Nano-silica microspheres are widely used in coatings, chromatographic column fillers, additives, etc. due to their high mechanical strength, good stability, and easy dispersion in solvents. At the same time, silica microspheres also have the advantages of non-toxicity, high biological activity, hydrophilicity, and easy functionalization of surface silicon light groups, so they have great application value in the fields of catalysts, biology, and medicine. In order to achieve a wider application of silica microspheres, silica fluorescent microspheres can be prepared by giving them fluorescent functions. Commonly used fluorescent dyes, such as naphthalene imide, fluorescein, and rhodamine dyes, are often used to prepare fluorescent balls. Among them, 1,8-naphthalene imide is famous for its typical intramolecular charge transfer (ICT) fluorophore, strong absorption and emission in the visible region, high photostability, and large Stokes shift. Using the corresponding 1,8-naphthoic anhydride as a raw material, naphthalene imide is synthesized by reacting with amines on the anhydride ring, and naphthalene imide is synthesized by reacting with the 4-position of the 4-naphthalene imide ring. Therefore, a series of derivatives can be produced for different applications. Fluorescent microspheres can be used as markers due to their stable structure, high luminescence efficiency and good dispersibility, and play an important role in the fields of composite microscopic detection, biological detection imaging, drug delivery and detection. Compared with traditional organic fluorescent molecules, the emission spectrum of rare earth ions is symmetrically distributed and narrow, not easy to photobleach, and has a long fluorescence lifetime and luminescence properties that do not change with the matrix material, so they are receiving more and more attention and research. Therefore, rare earth-doped fluorescent microspheres with silica as the matrix can be used as signal markers or fluorescent molecules to play an important role in the fields of composite microscopic detection, life analysis science and pharmaceutical targeted research.

[0004] In summary, the inorganic-organic composite fluorescent silica microspheres involved in the present invention have the characteristics of narrow particle size distribution range, simple synthesis, good dispersibility, strong fluorescence emission, etc. Summary of the invention

[0005] In view of the deficiencies of the prior art, the inventors have conducted intensive research. One of the purposes of the present invention is to provide an organic-inorganic composite fluorescent microsphere with uniform particle size and a preparation method thereof. The preparation method provided by the present invention not only simplifies the preparation process and reduces the cost of the luminescent material, but also can effectively control the fluorescence intensity of the microspheres. The obtained fluorescent microspheres have uniform particle size, high fluorescence efficiency, stable chemical properties, are environmentally friendly and have a simple preparation process. The most direct application is to prepare light-emitting devices by doping in materials, and can also be applied to ion detection, composite material microscopic detection, etc.

[0006] In order to achieve the above object, the present invention adopts the following technical scheme:

[0007] Naphthalene imide dyes were modified by solvothermal method to generate new silane coupling agents with both high fluorescence function and hydrolysis function of silane coupling agents. Nanosilica surface is rich in silanol (Si-OH) functions and can be modified to attach suitable fluorescent units. High surface area and availability of surface silanol functional groups allow high-density covalent immobilization of fluorescent coupling agents. This in turn helps in converting sensing events into higher responses in optical diagnostic applications and in the protection of signal molecules with optical transparency in the visible light region.

[0008] As a preferred technical solution of the present invention, a method for preparing a novel organic-inorganic composite fluorescent silica nanospheres comprises the following steps:

[0009] (1) 4-bromo-1,8-naphthalene dicarboxylic anhydride and n-butylamine were completely dissolved in ethanol, and then the mixture was subjected to a solvothermal reaction at 80° C. under a nitrogen atmosphere. After the reaction was completed, the mixture was cooled to room temperature and filtered. The filter cake was washed three times with ethanol and water respectively, and the crude product was recrystallized from ethanol and dried to obtain a white solid compound I;

[0010] (2) Add ethylenediamine to a three-necked flask equipped with a mechanical stirrer and a reflux condenser. Stir continuously at 50°C and evenly add compound I. Continue the reaction at the same temperature. After the reaction is completed, cool the mixture to room temperature and pour it into 30 ml of ice water. Filter the precipitate, wash with water, dry it, and recrystallize it from acetone to obtain orange solid compound II.

[0011] (3) Add the obtained compound II and isocyanosilane coupling agent (ICPTES) to anhydrous acetonitrile and react under nitrogen atmosphere and room temperature. Use triethylamine to catalyze the reaction. After the reaction is completed, evaporate the solvent, recrystallize the crude product from anhydrous acetonitrile, and then dry it with a vacuum pump to obtain a yellow solid compound III;

[0012] (4) The above compound III was transferred into a 50 mL single-necked flask, anhydrous ethanol was added for ultrasonic dissolution, and the pH was adjusted to 7 by ammonia water to obtain solution a. In addition, the nano-silica activated at high temperature was ultrasonically dispersed in an ethanol aqueous solution to obtain solution b. Solution a was added dropwise to solution b and mixed, and the mixture was stirred to react until a yellow emulsion was formed, and the supernatant was removed by centrifugation, and then washed with alcohol and centrifuged, vacuum dried, and crushed to obtain yellow fluorescent nano-silica microspheres.

[0013] Furthermore, in step (1), the 4-bromo-1,8-naphthalene dicarboxylic anhydride and n-butylamine are in a molar ratio of 1:1.3.

[0014] Furthermore, the solvent thermal reaction time in step (1) is more than 6 hours.

[0015] Furthermore, in step (2), the molar ratio of compound I to ethylenediamine is 1:62.

[0016] Furthermore, the compound I in step (2) needs to be added within 1 hour and the total reaction time is more than 5 hours.

[0017] Furthermore, in step (3), the molar ratio of compound II to isocyanosilane coupling agent is 1:1.05; and the reaction time is more than 2 hours.

[0018] Furthermore, in step (4), the ratio of compound III to nano-silicon dioxide is 0.3 mmol:4 g.

[0019] Furthermore, the volume ratio of ethanol to water in the ethanol-water solution in step (4) is 3:1.

[0020] Furthermore, in step (4), the stirring temperature is 50° C. and the stirring time is 3 h.

[0021] Furthermore, in step (4), the centrifugal speed is ≥8000 rpm, and the centrifugal time is 4 min or longer. Wash with ethanol several times, use an oscillator to mix the solution evenly, and then centrifuge until the supernatant is transparent.

[0022] Beneficial effects of the present invention: Compared with the prior art, the present invention has the following advantages:

[0023] 1. The fluorescent silica nanospheres prepared by the method of the present invention have the advantages of good dispersibility, large specific surface area, high fluorescence intensity and stability compared with single probes, can be directly doped in silica gel rubber to make fluorescent devices, and can also be used for ion detection and observation of the spatial distribution structure of silica in polymers.

[0024] 2. The fluorescent silica nanoparticles prepared by the method of the present invention have excellent non-toxicity and biocompatibility, and can be widely used in the fields of biological analysis, fluorescence imaging and material analysis;

[0025] 3. The fluorescent silica nanospheres prepared by the method of the present invention have a unique spherical structure and a long fluorescence lifetime, and will have potential application value in other fields in the future.

[0026] 4. The preparation process of the method of the present invention is simple, does not require a complicated purification process, saves time and labor, and the prepared nanoparticles do not require other treatments. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a physical picture of the silane coupling agent-naphthaleneimide fluorescent dye ethanol solution prepared in Example 1 of the present invention under sunlight and ultraviolet light.

[0028] Figure 2 The silane coupling agent-naphthalimide fluorescent dye prepared in Example 1 of the present invention 1 H NMR spectrum.

[0029] Figure 3 It is a fluorescence emission spectrum diagram of ethanol solutions of yellow-green fluorescent dye with different concentration gradients prepared in Example 1 of the present invention.

[0030] Figure 4 This is a picture of the fluorescent silica nanospheres prepared in Example 1 of the present invention under a fluorescence microscope.

[0031] Figure 5 This is a SEM image of the yellow fluorescent silica nanospheres prepared in Example 1 of the present invention.

[0032] Figure 6 This is a physical picture of the fluorescent silica nanospheres prepared in Example 1 of the present invention under sunlight and ultraviolet light.

[0033] Figure 7 This is a schematic diagram showing the effect of different amounts of triethylamine on the reaction completion time for obtaining silane coupling agent-naphthaleneimide fluorescent dye.

[0034] Figure 8 is the fluorescence intensity of fluorescent silica nanospheres obtained at different reaction times.

[0035] Fig. 9 is the fluorescence intensity of fluorescent silica nanospheres obtained at different reaction temperatures. DETAILED DESCRIPTION

[0036] To make the purpose, technical scheme and advantages of the present invention clearer, the specific embodiments of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The present invention is not limited to the materials, reaction conditions or parameters mentioned in these embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.

[0037] The above scheme is further described below in conjunction with specific implementation examples. The preferred embodiments of the present invention are described in detail as follows:

[0038] Example 1: This embodiment provides a novel method for preparing organic-inorganic composite fluorescent silica nanospheres, which is achieved by the following steps:

[0039] (1) 4-Bromo-1,8-naphthalene dicarboxylic anhydride (5.000 g, 18.000 mmol) and n-butylamine (1.700 g, 23.400 mmol) were completely dissolved in 70 mL of ethanol and refluxed for 6 h under a nitrogen atmosphere. After the reaction was completed, the mixture was cooled to room temperature and filtered. The filter cake was washed three times with ethanol and water respectively, and the crude product was recrystallized from ethanol and dried to obtain 4.832 g of white solid N-n-butyl-4-bromo-1,8-naphthalene dicarboxylic anhydride (Compound I), with a yield of 80.6%;

[0040] (2) Add 10 ml of ethylenediamine to a three-necked flask equipped with a mechanical stirrer and a reflux condenser. Stir continuously at 50°C for 1 hour, and evenly add compound I (0.800 g, 2.410 mmol). After heating at the same temperature for 4 hours, cool the mixture to room temperature and pour it into 20 ml of ice water. Filter the precipitate, wash it three times with 100 mL of water, dry it, and recrystallize it from acetone to obtain 0.588 g of orange solid N-n-butyl-4-ethylenediamino-1,8-naphthalic anhydride (compound II), with a yield of 78.3%;

[0041] (3) Compound II (0.623 g, 2 mmol) was dissolved in 60 mL of anhydrous acetonitrile, and 3 drops of triethylamine were added to catalyze the reaction. At room temperature and in an inert atmosphere, isocyanosilane coupling agent (ICPTES) (552.6 uL, 2.12 mmol) was added with a syringe, and the reaction was stirred magnetically for 2 h. The solvent was evaporated, and then dried with a vacuum pump for 1 h, and finally 1.0833 g of a yellow solid (Compound III) was obtained, with a yield of 92%.

[0042] (4) The above 0.3 mmol of compound III was transferred into a 50 mL single-necked flask, 15 mL of anhydrous ethanol was added for ultrasonic dissolution and the pH was adjusted to 7 by ammonia water to obtain solution a. In addition, the nano-silica activated at high temperature was dissolved in 100 mL of ethanol aqueous solution (ethanol: water = 3:1) and ultrasonically dispersed for 30 min to obtain solution b. Solution a was added dropwise to solution b, the reaction temperature was controlled to 50 ° C, and magnetic stirring was performed for 3 h. The obtained solution was centrifuged at 8500 rpm for 5 min to remove the supernatant, and then washed and centrifuged three times with deionized water and anhydrous ethanol respectively. Finally, the obtained yellow product was placed in a 75 ° C oven to dry to constant weight, and fluorescent nano-silica microspheres were obtained.

[0043] Figure 1 The following are the actual pictures of the silane coupling agent-naphthalimide fluorescent dye ethanol solution prepared in Example 1 of the present invention under sunlight and ultraviolet light. It can be seen from the picture that the silane coupling agent-naphthalimide fluorescent dye has fluorescent properties.

[0044] Figure 2The silane coupling agent-naphthalimide fluorescent dye prepared in Example 1 of the present invention 1 H NMR spectrum.

[0045] Figure 3 It is a fluorescence emission spectrum diagram of ethanol solutions of yellow-green fluorescent dye with different concentration gradients prepared in Example 1 of the present invention.

[0046] Figure 4 This is a picture of the fluorescent silica nanospheres prepared in Example 1 of the present invention under a fluorescence microscope. It can be seen that the prepared silica microspheres are spheres of about 100 nm.

[0047] Figure 5 This is a SEM image of the yellow fluorescent silica nanospheres prepared in Example 1 of the present invention.

[0048] Figure 6 This is a physical picture of the fluorescent silica nanospheres prepared in Example 1 of the present invention under sunlight and ultraviolet light.

[0049] Example 2

[0050] This example is similar to Example 1, except that the amount of n-butylamine added in step (1) is 1.448 g. The yield of the obtained compound I is slightly lower than that of Example 1.

[0051] Example 3

[0052] This example is similar to Example 1, except that the amount of n-butylamine added in step (1) is 1.843 g. The yield of the obtained compound I is slightly lower than that of Example 1.

[0053] Example 4

[0054] This example is similar to Example 1, except that the ratio of anhydrous ethanol to compound I in step (1) is 150 ml:1 g. The yield of compound I is lower than that in Example 1.

[0055] Example 5

[0056] This example is similar to Example 1, except that the amount of ethylenediamine added in step (2) is 5 ml, 15 ml, and 20 ml. The different amounts of ethylenediamine added affect the yield of compound II but do not affect the properties of the product.

[0057] Example 6

[0058] This example is substantially the same as Example 1, except that the amount of anhydrous acetonitrile used in step (3) is 40 ml, 50 ml, 70 ml, and 80 ml. Different amounts of anhydrous acetonitrile used affect the yield of compound II without affecting the properties of the product, with the yield of 80 ml being the lowest.

[0059] Example 7

[0060] This embodiment is substantially the same as embodiment 1, except that the amount of triethylamine used in step (3) is changed from 3 drops to 0, 1, 4, 6, and 8 drops, respectively. When the amount of triethylamine used is too small, it will affect the catalytic efficiency and thus the reaction completion time. When the content is too high, there is no effect. Figure 7 The preferred dosage is 2-8 drops, and the optimal dosage is 3 drops. As a base, triethylamine does not affect the structure of the fluorescent dye at a higher pH value, indicating that the reaction has good stability.

[0061] Example 8

[0062] This embodiment is roughly the same as embodiment 1, except that the stirring time in step (4) is changed from 3 hours to 30 minutes, 1 hour, 2 hours, 4 hours, and 5 hours respectively. Other aspects are the same as embodiment 1. The stirring time affects the loading rate of the fluorescent dye on the silica nanospheres, and thus affects the fluorescence performance. When the reaction time exceeds 2 hours, further increasing the reaction time does not significantly improve the fluorescence intensity, indicating that the reaction time is 2 hours during the fluorescent labeling process, and the reaction process is basically completed, and the enhancement of the fluorescence effect is consistent with the degree of reaction. Figure 8 As shown in the figure, it can be seen that the preferred stirring time is 2-3h, and the optimal stirring time is 2h.

[0063] Example 9

[0064] This embodiment is substantially the same as embodiment 1, except that the stirring temperature in step (4) is changed from 50°C to 20, 30, 40, 60, and 70°C, respectively. As the reaction temperature increases by 20-70°C, the fluorescence intensity also changes accordingly. Fig. 9 As shown in the figure, it can be seen that the preferred stirring time is 50-70°C with a stronger fluorescence intensity, and the optimal stirring temperature is 70°C.

[0065] The above embodiments of the present invention are described in detail in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments, and various changes can be made according to the purpose of the invention of the present invention. Any changes, modifications, substitutions, combinations or simplifications made according to the spirit and principle of the technical solution of the present invention should be equivalent replacement methods, which all fall within the scope of the present invention. Those of ordinary skill in the art should understand that many changes can be made within the spirit of the present invention and the scope of the current or future claims.

Claims

1. A method for preparing inorganic-organic composite fluorescent silica microspheres, characterized in that: The steps include: (1) 4-bromo-1,8-naphthalene dicarboxylic anhydride and n-butylamine were completely dissolved in ethanol, and then the mixture was subjected to a solvothermal reaction at 80° C. under a nitrogen atmosphere. After the reaction was completed, the mixture was cooled to room temperature and filtered. The filter cake was washed three times with ethanol and water respectively, and the crude product was recrystallized from ethanol and dried to obtain a white solid compound I; (2) Add ethylenediamine to a three-necked flask equipped with a mechanical stirrer and a reflux condenser. Stir continuously at 50°C and evenly add compound I. Continue the reaction at the same temperature. After the reaction is completed, cool the mixture to room temperature and pour it into 30 ml of ice water. Filter the precipitate, wash with water, dry it, and recrystallize it from acetone to obtain orange solid compound II. (3) Add the obtained compound II and isocyanosilane coupling agent (ICPTES) to anhydrous acetonitrile and react under nitrogen atmosphere and room temperature. Use triethylamine to catalyze the reaction. After the reaction is completed, evaporate the solvent, recrystallize the crude product from anhydrous acetonitrile, and then dry it with a vacuum pump to obtain a yellow solid compound III; (4) The above compound III was transferred into a 50 mL single-necked flask, anhydrous ethanol was added for ultrasonic dissolution, and the pH was adjusted to 7 by ammonia water to obtain solution a. In addition, the nano-silica activated at high temperature was ultrasonically dispersed in an ethanol aqueous solution to obtain solution b. Solution a was added dropwise to solution b and mixed, and the mixture was stirred to react until a yellow emulsion was formed, and the supernatant was removed by centrifugation, and then washed with alcohol and centrifuged, vacuum dried, and crushed to obtain yellow fluorescent nano-silica microspheres.

2. The preparation method according to claim 1, characterized in that In step (1), the 4-bromo-1,8-naphthalene dicarboxylic anhydride and n-butylamine are in a molar ratio of 1:1.

3.

3. The preparation method according to claim 1, characterized in that The solvent thermal reaction time of step (1) is more than 6 hours.

4. The preparation method according to claim 1, characterized in that In step (2), the molar ratio of compound I to ethylenediamine is 1:

62.

5. The preparation method according to claim 1, characterized in that In step (2), the compound I must be added within 1 hour and the total reaction time is more than 5 hours.

6. The preparation method according to claim 1, characterized in that In step (3), the compound II and the isocyanosilane coupling agent are in a molar ratio of 1:1.05; and the reaction time is more than 2 hours.

7. The preparation method according to claim 1, characterized in that In step (4), the ratio of compound III to nano-silicon dioxide is 0.3 mmol:4 g.

8. The preparation method according to claim 1, characterized in that The volume ratio of ethanol to water in the ethanol-water solution of step (4) is 3:

1.

9. The preparation method according to claim 1, characterized in that The stirring temperature in step (4) is 50° C. and the stirring time is 3 h.

10. The preparation method according to claim 1, characterized in that In step (4), the centrifugal speed is ≥8000 rpm, and the centrifugal time is 4 min or longer. Wash with ethanol several times, use an oscillator to mix the solution evenly, and then centrifuge until the supernatant is transparent.

Citation Information

Cited By

  • Fluorescent hollow glass bead and preparation method thereof

    CN121379569A