Prefabricating method and application of longitudinal cracks of environmental barrier coating

By processing microstructures on the surface of the ceramic matrix and forming longitudinal cracks with specific coating deposition methods, the problem of the ceramic matrix composite coating is easily corroded in high-temperature water-oxygen environments is solved, and the bonding strength between the coating and the substrate is significantly improved. Thermal shock resistance meets the needs of high temperature stability and thermal shock resistance.

CN118895478AActive Publication Date: 2024-11-05GUANGDONG INST OF NEW MATERIALS
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410907784.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-05
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

Ceramic matrix composite materials are easily corroded under high temperature water and oxygen environment. During the spraying and preparation process, the rare earth silicate coating has low bond strength and is easy to peel off due to stress problems, which cannot meet the needs of high temperature stability and thermal shock resistance. .

Method used

Process microstructures of specific shapes, such as U-shaped straight grooves, V-shaped straight grooves or U-shaped blind holes, and form longitudinal cracks in the microstructure through plasma spray-physical vapor deposition method, releasing stresses generated during the deposition process , improve the bond strength between the coating and the substrate.

Benefits of technology

It significantly improves the bonding strength between the coating and the substrate, prevents the coating from falling off during the preparation process, and maintains good thermal shock resistance in high-temperature environments, meets the later service requirements, and the bonding strength is higher than that of traditional sandblasting coarse technology. 2.1-3.6 times.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895478A_ABST
    Figure CN118895478A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of coatings, and particularly relates to a prefabrication method and application of longitudinal cracks of an environmental barrier coating. The prefabrication method for the longitudinal cracks of the environmental barrier coating comprises the following steps that a microstructure is machined on the surface of a base body, then the coating is deposited, and the longitudinal cracks are formed in the coating; the microstructure comprises a plurality of U-shaped straight grooves, a plurality of V-shaped straight grooves or a plurality of U-shaped blind holes; the method for depositing the coating comprises any one of plasma spraying-physical vapor deposition and low-pressure plasma spraying. According to the method, the microstructure in a specific shape is machined on the surface of the base body, and a specific coating deposition method is combined, so that the bonding strength of the coating and the base material can be improved, and the coating is prevented from falling off in the preparation process. Besides, the sample containing the longitudinal cracks is subjected to high-temperature annealing treatment, so that healing of the longitudinal cracks can be promoted, the situation that the coating loses efficacy in advance due to the fact that corrosive substances permeate into the coating in the service process is prevented, and the later service requirement can be well met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and in particular relates to a method for prefabricating longitudinal cracks of an environmental barrier coating and its application. Background Art

[0002] Environmental barrier coating is a type of high-temperature protective coating for the hot end components of aircraft engines. It is coated on the surface of ceramic-based composite structural components of aircraft engines. Its function is to establish a barrier between the ceramic-based composite structural components and the harsh working environment, preventing or reducing the negative impact of high temperature environment on component performance.

[0003] The inlet temperature of the turbine of an aircraft engine is high, and accordingly, its hot end components are required to have better high-temperature stability and thermal shock resistance. Ceramic matrix materials have become the preferred materials for hot end components of aircraft engines due to their advantages such as high temperature resistance, low density and high strength. However, since ceramic matrix materials are easily corroded in high-temperature water and oxygen environments (up to 1350°C), rare earth silicate coatings must be coated on their surfaces to protect them from corrosion by high-temperature water and oxygen and external sediments, and effectively block the penetration of high-temperature water and oxygen and external corrosive substances to achieve a protective effect on the ceramic matrix materials. However, during the spraying preparation process of the rare earth silicate coating, due to the stress problem inside the coating, the bonding strength between the coating and the ceramic matrix material is low, and the coating is even easy to peel off during the spraying preparation process, which cannot meet the subsequent service requirements.

[0004] Therefore, it is of great significance to provide a method that can effectively release the stress generated during the deposition process of the coating, reduce the internal stress of the coating, thereby improving the bonding strength between the coating and the substrate and preventing the coating from falling off during the preparation process. Summary of the invention

[0005] The present invention aims to solve one or more technical problems existing in the above-mentioned prior art, and at least provide a beneficial choice or create conditions. Specifically, the present invention provides a method for prefabricating longitudinal cracks in an environmental barrier coating, which can effectively release the stress generated during the deposition process of the coating, reduce the internal stress of the coating, and thus improve the bonding strength between the coating and the substrate, and prevent the coating from falling off during the preparation process.

[0006] The inventive concept of the present invention: The prefabrication method of the longitudinal cracks of the environmental barrier coating of the present invention comprises the following steps: processing a microstructure on the surface of the substrate, then depositing the coating, and forming a longitudinal crack in the coating; the microstructure comprises a plurality of U-shaped straight grooves, a plurality of V-shaped straight grooves or a plurality of U-shaped blind holes; the method of depositing the coating comprises any one of plasma spraying-physical vapor deposition and low-pressure plasma spraying. The present invention improves the bonding strength between the coating and the substrate by processing a microstructure of a specific shape on the surface of the substrate and combining a specific coating deposition method. The microstructure can adjust the internal stress of the coating, especially for high-density environmental barrier coatings. The coating deposited at the position of the microstructure groove generates a compressive stress in the surface, while the position of the microstructure protrusion generates a tensile stress in the surface. The tensile stress and the compressive stress are mutually controlled. Prefabricated microcracks are formed at or near the position of the microstructure protrusion, which can effectively release the stress generated during the coating deposition process, reduce the internal stress of the coating, increase the strain tolerance of the coating, and improve the success rate of depositing the coating in combination with a specific coating deposition method, improve the bonding strength between the coating and the substrate, and prevent the coating from falling off during the preparation process. The bonding strength between the coating with longitudinal cracks and the substrate of the present invention is significantly higher than the bonding strength between the coating prepared by the traditional sandblasting roughening technology and the substrate, which is 2.1-3.6 times that of the traditional sandblasting roughening technology.

[0007] Therefore, a first aspect of the present invention provides a method for prefabricating longitudinal cracks in an environmental barrier coating.

[0008] Specifically, the method for prefabricating longitudinal cracks in the environmental barrier coating comprises the following steps:

[0009] The microstructure is machined on the substrate surface, and then the coating is deposited to form longitudinal cracks in the coating;

[0010] The microstructure includes a plurality of U-shaped straight grooves, a plurality of V-shaped straight grooves or a plurality of U-shaped blind holes;

[0011] The coating deposition method includes any one of plasma spraying-physical vapor deposition and low-pressure plasma spraying.

[0012] Specifically, the “multiple” in the multiple U-shaped straight grooves, multiple V-shaped straight grooves or multiple U-shaped blind holes refers to two or more.

[0013] Preferably, the matrix comprises silicon carbide ceramics, silicon carbide fiber reinforced silicon carbide (SiC f / SiC) ceramic matrix composites, carbon fiber reinforced silicon carbide (C f / SiC) ceramic matrix composite material.

[0014] Preferably, a laser is used to process the surface of the substrate to form a microstructure.

[0015] Preferably, the laser includes any one of a millisecond laser, a nanosecond laser, a picosecond laser and a femtosecond laser; further preferably, the laser includes a femtosecond laser.

[0016] Preferably, the process parameters of the femtosecond laser for processing microstructures are as follows: laser power is 4.4-22W, repetition frequency is 9-110KHz, scanning speed is 0.45-22mm / s, number of scanning passes is 1-22 times, scanning spacing is 0.1-1.1mm, and defocus is greater than or equal to -2.2mm and less than or equal to 2.2mm.

[0017] Further preferably, the process parameters of the femtosecond laser for processing microstructures are as follows: laser power is 5-20W, repetition frequency is 10-100KHz, scanning speed is 0.5-20mm / s, number of scanning times is 1-20 times, scanning spacing is 0.1-1mm, and defocus is greater than or equal to -2mm and less than or equal to 2mm.

[0018] Preferably, the substrate needs to be ultrasonically cleaned before and after the microstructure is processed.

[0019] Preferably, the detergent for ultrasonic cleaning includes at least one of anhydrous ethanol and acetone.

[0020] Preferably, the ultrasonic cleaning time is 25-35 min; further preferably, the ultrasonic cleaning time is 27-33 min; further preferably, the ultrasonic cleaning time is 30 min.

[0021] Preferably, the environment in which the microstructure is processed on the surface of the substrate by using a laser includes any one of a solution environment, an inert gas environment and an atmospheric environment.

[0022] Preferably, the width of the U-shaped straight groove is 55μm-330μm, the depth of the U-shaped straight groove is 18μm-220μm, and the spacing between two adjacent U-shaped straight grooves is 0μm-550μm; further preferably, the width of the U-shaped straight groove is 60μm-300μm, the depth of the U-shaped straight groove is 20μm-200μm, and the spacing between two adjacent U-shaped straight grooves is 50μm-300μm.

[0023] Preferably, the width of the V-shaped straight groove is 45μm-550μm, the depth of the V-shaped straight groove is 27μm-330μm, and the spacing between two adjacent V-shaped straight grooves is 0μm-550μm; further preferably, the width of the V-shaped straight groove is 50μm-500μm, the depth of the V-shaped straight groove is 30μm-300μm, and the spacing between the V-shaped straight grooves is 50μm-300μm.

[0024] Preferably, the diameter of the U-shaped blind hole is 65μm-880μm, the depth of the U-shaped blind hole is 18μm-330μm, and the spacing between two adjacent U-shaped blind holes in the X direction is 9μm-550μm; the spacing between two adjacent U-shaped blind holes in the Y direction is 9μm-550μm; further preferably, the diameter of the U-shaped blind hole is 70μm-800μm, the depth of the U-shaped blind hole is 20μm-300μm, and the spacing between two adjacent U-shaped blind holes in the X direction is 10μm-500μm; the spacing between two adjacent U-shaped blind holes in the Y direction is 10μm-500μm.

[0025] Preferably, the microstructure comprises a plurality of U-shaped blind holes.

[0026] Preferably, the method of depositing the coating comprises plasma spray-physical vapor deposition.

[0027] Preferably, the process conditions of the plasma spraying-physical vapor deposition are as follows: spraying distance is 750-1300 mm, current is 2200-3000 A, argon gas flow rate is 80-120 L / min, and substrate preheating temperature is 750-1100°C.

[0028] Further preferably, the process conditions of the plasma spraying-physical vapor deposition are as follows: the spraying distance is 800-1200 mm, the current is 2500-2700 A, the argon gas flow rate is 90-110 L / min, and the substrate preheating temperature is 800-1000°C.

[0029] Preferably, the coating comprises Re 2 Si 2 O 7 、Re 2 SiO 5 Any one of; the Re includes any one of Yb, Y, Sc, Lu, and Er.

[0030] Preferably, the coating comprises Yb 2 Si 2 O 7 .

[0031] Specifically, the coating is a rare earth silicate coating.

[0032] Preferably, when the coating is deposited, the particle size of the rare earth silicate is 13-80 μm; further preferably, when the coating is deposited, the particle size of the rare earth silicate is 15-75 μm.

[0033] Preferably, the thickness of the coating is 45-220 μm; further preferably, the thickness of the coating is 50-200 μm.

[0034] Preferably, the width of the longitudinal crack is 200 nm-3.3 μm; further preferably, the width of the longitudinal crack is 300 nm-3 μm.

[0035] A second aspect of the present invention provides an engine.

[0036] Specifically, the engine includes a coating prepared by the method for prefabricating longitudinal cracks in an environmental barrier coating according to the first aspect of the present invention.

[0037] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:

[0038] (1) The present invention improves the bonding strength between the coating and the substrate by processing a microstructure of a specific shape on the surface of the substrate and combining a specific coating deposition method. The microstructure can adjust the internal stress of the coating. Especially for high-density environmental barrier coatings, the coating deposited at the groove position of the microstructure generates compressive stress in the surface, while the protruding position of the microstructure generates tensile stress in the surface. The tensile stress and compressive stress are mutually dependent, and prefabricated microcracks are formed at or near the protruding position of the microstructure, which can effectively release the stress generated during the coating deposition process, reduce the internal stress of the coating, increase the strain tolerance of the coating, and combine with a specific coating deposition method to improve the success rate of the deposited coating, thereby improving the bonding strength between the coating and the substrate and preventing the coating from falling off during the preparation process. The bonding strength between the coating with longitudinal cracks and the substrate of the present invention is significantly higher than the bonding strength between the coating and the substrate prepared by the traditional sandblasting roughening technology, which is 2.1-3.6 times that of the traditional sandblasting roughening technology.

[0039] (2) The present invention uses a laser to process a low-damage microstructure on the surface of the substrate. The microstructure is evenly distributed and can replace the traditional sandblasting method to improve the bonding strength between the coating and the substrate. Since the hardness of ceramic materials is relatively high, it is difficult to obtain a rough surface by using the traditional sandblasting method, and excessive sandblasting pressure will damage the ceramic substrate.

[0040] (3) After longitudinal cracks are obtained, the present invention can promote the healing of longitudinal cracks by performing high-temperature annealing treatment on the sample containing longitudinal cracks, thereby preventing corrosive substances from penetrating into the coating during service and causing premature failure of the coating. After the longitudinal cracks are healed, the coating still has good thermal shock resistance and can well meet the later service requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is a scanning electron microscope image of the surface morphology of the silicon carbide ceramic substrate surface microstructure of Example 1 of the present invention;

[0042] Figure 2 This is a scanning electron microscope image of a cross section of the environmental barrier coating prepared in Example 1 of the present invention;

[0043] Figure 3 This is a scanning electron microscope image of a cross section of an environmental barrier coating prepared in Comparative Example 1 of the present invention;

[0044] Figure 4 This is a scanning electron microscope image of the cross section of the environmental barrier coating after the longitudinal crack of Example 1 of the present invention has been healed. DETAILED DESCRIPTION

[0045] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.

[0046] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0047] Example 1

[0048] A method for prefabricating longitudinal cracks in an environmental barrier coating comprises the following steps:

[0049] (1) The silicon carbide ceramic sample is placed in a beaker filled with anhydrous ethanol, ultrasonically cleaned for 30 minutes, and then placed in a fixture filled with deionized water, the position of the silicon carbide ceramic substrate is adjusted, the water film thickness is maintained at 0.5 mm, and a femtosecond laser is used to process a U-shaped straight groove structure on the surface of the silicon carbide ceramic substrate. The process parameters are: laser power of 10 W, repetition frequency of 50 KHz, scanning speed of 1 mm / s, scanning times of 5 times, scanning spacing of 0.2 mm, defocusing amount of -1 mm, and processing environment of deionized water solution. The width of the processed U-shaped straight groove is 150 μm, the depth of the U-shaped straight groove is 80 μm, and the spacing between two adjacent U-shaped straight grooves is 160 μm; the processed silicon carbide ceramic substrate is placed in a beaker filled with anhydrous ethanol and ultrasonically cleaned for 30 minutes to obtain a silicon carbide ceramic substrate with a processed microstructure;

[0050] (2) Using a plasma spray-physical vapor deposition method to prepare Yb on the microstructured silicon carbide ceramic substrate obtained in step (1) 2 Si 2 O 7 Coating, plasma spray-physical vapor deposition process parameters are: spray distance 1000mm, current 2600A, argon flow rate 110L / min, substrate preheating temperature 800℃; preparation raw materials (Yb 2 Si 2 O 7 ) has a particle size range of 15-45 μm. The sprayed sample is air-cooled in a plasma spray-physical vapor deposition device to obtain a silicon carbide ceramic with a deposited coating.

[0051] Example 1 Surface morphology scanning electron microscope image of the surface microstructure of the silicon carbide ceramic substrate is as follows Figure 1 shown.

[0052] The cross section of the environmental barrier coating prepared in Example 1 was observed by scanning electron microscopy, and the results were as follows: Figure 2 As shown. Figure 2 It can be seen that Yb 2 Si 2 O 7 The coating successfully preformed longitudinal microcracks at the raised positions between the microstructures due to the internal stress, with a crack width of 700nm-2μm. This is because the coating deposited at the groove position of the microstructure produces in-plane compressive stress, while the raised position of the microstructure produces in-plane tensile stress. The tensile and compressive stresses affect each other, forming microcracks at or near the raised position of the microstructure.

[0053] Example 2

[0054] A method for prefabricating longitudinal cracks in an environmental barrier coating comprises the following steps:

[0055] (1) SiC f The sample of the / SiC ceramic matrix composite material was placed in a beaker filled with anhydrous ethanol and ultrasonically cleaned for 30 min. It was then placed in a fixture and the SiC f / SiC ceramic matrix composite sample position, using femtosecond laser to f The V-shaped straight groove structure was processed on the surface of the SiC ceramic matrix composite material. The process parameters were as follows: laser power of 10W, repetition frequency of 50KHz, scanning speed of 5mm / s, scanning times of 5 times, scanning spacing of 0.2mm, defocus of -1mm, and processing environment of atmospheric environment. The width of the processed V-shaped straight groove was 90μm, the depth of the V-shaped straight groove was 170μm, and the spacing between two adjacent V-shaped straight grooves was 200μm. The processed SiC f The matrix of the SiC ceramic matrix composite material was placed in a beaker filled with anhydrous ethanol and ultrasonically cleaned for 30 minutes to obtain the SiC ceramic matrix with microstructure. f / SiC ceramic matrix composite material matrix;

[0056] (2) Using a plasma spray-physical vapor deposition method to process the microstructured SiC obtained in step (1) f Preparation of Yb on SiC ceramic matrix composites 2 Si 2 O 7 The process parameters of plasma spraying-physical vapor deposition are as follows: spraying distance is 1000 mm, current is 2600 A, argon gas flow rate is 110 L / min, substrate preheating temperature is 800 °C; preparation raw materials (Yb 2Si 2 O 7 ) has a particle size range of 15-45 μm. The sprayed samples are air-cooled in a plasma spray-physical vapor deposition device to obtain a deposited SiC coating. f / SiC ceramic matrix composite materials.

[0057] Yb 2 Si 2 O 7 Due to the internal stress, longitudinal microcracks are successfully preformed at the raised positions between the microstructures inside the coating, and the crack width is 700nm-1.5μm.

[0058] Example 3

[0059] A method for prefabricating longitudinal cracks in an environmental barrier coating comprises the following steps:

[0060] (1) C f The matrix of the / SiC ceramic matrix composite material was placed in a beaker filled with anhydrous ethanol and ultrasonically cleaned for 30 min. It was then placed in a fixture filled with inert gas and the C f / SiC ceramic matrix composite matrix position, to maintain the airtightness of the device, a femtosecond laser was used to f The surface of the SiC ceramic matrix composite material was processed with V-shaped straight groove structure. The process parameters were: laser power of 10W, repetition frequency of 50KHz, scanning speed of 5mm / s, number of scanning passes of 5 times, scanning spacing of 0.2mm, defocus of -1mm, and processing environment of N 2 Environment, the width of the processed V-shaped straight groove is 80μm, the depth of the V-shaped straight groove is 150μm, and the distance between two adjacent V-shaped straight grooves is 220μm; f The sample of the C / SiC ceramic matrix composite material was placed in a beaker filled with anhydrous ethanol and ultrasonically cleaned for 30 min to obtain a C / SiC ceramic matrix composite material with a microstructure. f / SiC ceramic matrix composite material matrix;

[0061] (2) Plasma spray-physical vapor deposition method is used to process the microstructured C obtained in step (1) f Preparation of Yb / SiC ceramic matrix composite matrix 2 Si 2 O 7 The process parameters of plasma spraying-physical vapor deposition are as follows: spraying distance is 1000 mm, current is 2600 A, argon gas flow rate is 110 L / min, substrate preheating temperature is 800 °C; preparation raw materials (Yb 2 Si 2 O 7) with a particle size range of 15-45 μm. The sprayed samples were air-cooled in a plasma spray-physical vapor deposition device to obtain the C f / SiC ceramic matrix composite materials.

[0062] Yb 2 Si 2 O 7 Due to the internal stress, longitudinal microcracks are successfully preformed at the raised positions between the microstructures inside the coating, and the crack width is 800nm-1.5μm.

[0063] Example 4

[0064] A method for prefabricating longitudinal cracks in an environmental barrier coating comprises the following steps:

[0065] (1) SiC f The matrix of the / SiC ceramic matrix composite material was placed in a beaker filled with anhydrous ethanol and ultrasonically cleaned for 30 min. It was then placed in a fixture filled with deionized water to adjust the SiC f / SiC ceramic matrix composite matrix, keeping the water film thickness at 0.5mm, and using femtosecond laser to f The U-shaped blind hole microstructure was processed on the surface of SiC ceramic matrix composite material. The process parameters were as follows: laser power of 10W, repetition frequency of 50KHz, scanning speed of 1mm / s, scanning times of 5 times, scanning spacing of 0.2mm, defocusing amount of -1mm, and processing environment of deionized water solution. The diameter of the processed U-shaped blind hole was 150μm, the depth of the U-shaped blind hole was 90μm, and the spacing between two adjacent U-shaped blind holes in the X and Y directions was 60μm. The processed SiC f The sample of the / SiC ceramic matrix composite material was placed in a beaker filled with anhydrous ethanol and ultrasonically cleaned for 30 minutes to obtain the SiC with microstructure processed. f / SiC ceramic matrix composite material matrix;

[0066] (2) Using a plasma spray-physical vapor deposition method to process the microstructured SiC obtained in step (1) f Preparation of Yb on SiC ceramic matrix composites 2 Si 2 O 7 The process parameters of plasma spraying-physical vapor deposition are as follows: spraying distance is 1000 mm, current is 2600 A, argon gas flow rate is 110 L / min, substrate preheating temperature is 800 °C; preparation raw materials (Yb 2 Si 2 O 7) has a particle size range of 15-45 μm. The sprayed samples are air-cooled in a plasma spray-physical vapor deposition device to obtain a deposited SiC coating. f / SiC ceramic matrix composite materials.

[0067] Yb 2 Si 2 O 7 Due to the internal stress, longitudinal microcracks are successfully preformed at the raised positions between the microstructures inside the coating, and the crack width is 800nm-1.5μm.

[0068] Example 5

[0069] A method for prefabricating longitudinal cracks in an environmental barrier coating comprises the following steps:

[0070] (1) C f The matrix of the / SiC ceramic matrix composite material was placed in a beaker filled with anhydrous ethanol and ultrasonically cleaned for 30 min. It was then placed on a fixture and the C f The position of the matrix of the SiC ceramic matrix composite was determined by femtosecond laser. f The surface of the SiC ceramic matrix composite material was processed with V-shaped straight groove microstructure. The process parameters were as follows: laser power of 10W, repetition frequency of 50KHz, scanning speed of 1mm / s, scanning times of 5 times, scanning spacing of 0.2mm, defocus of -1mm, and processing environment of atmospheric environment. The width of the processed V-shaped straight groove was 75μm, the depth of the V-shaped straight groove was 130μm, and the spacing between two adjacent V-shaped straight grooves was 210μm. f The sample of the C / SiC ceramic matrix composite material was placed in a beaker filled with anhydrous ethanol and ultrasonically cleaned for 30 min to obtain a C / SiC ceramic matrix composite material with a microstructure. f / SiC ceramic matrix composite material matrix;

[0071] (2) Plasma spray-physical vapor deposition method is used to process the microstructured C obtained in step (1) f Preparation of Yb on SiC ceramic matrix composites 2 Si 2 O 7 The process parameters of plasma spraying-physical vapor deposition are as follows: spraying distance is 1000 mm, current is 2600 A, argon gas flow rate is 110 L / min, substrate preheating temperature is 800 °C; preparation raw materials (Yb 2 Si 2 O 7 ) with a particle size range of 15-45 μm. The sprayed samples were air-cooled in a plasma spray-physical vapor deposition device to obtain the C f / SiC ceramic matrix composite materials.

[0072] Yb 2 Si 2 O 7 Due to the internal stress, longitudinal microcracks are successfully preformed at the raised positions between the microstructures inside the coating, and the crack width is 700nm-1.5μm.

[0073] Example 6

[0074] A method for prefabricating longitudinal cracks in an environmental barrier coating comprises the following steps:

[0075] (1) The silicon carbide ceramic sample was placed in a beaker filled with anhydrous ethanol, ultrasonically cleaned for 30 minutes, and then placed in a fixture filled with deionized water. The position of the silicon carbide sample was adjusted to maintain the water film thickness of 0.5 mm. A femtosecond laser was used to process the U-shaped straight groove structure on the surface of the silicon carbide ceramic. The process parameters were: laser power of 10 W, repetition frequency of 50 KHz, scanning speed of 1 mm / s, scanning times of 5 times, scanning spacing of 0.2 mm, defocusing amount of -1 mm, and processing environment of deionized water solution. The width of the processed U-shaped straight groove was 150 μm, the depth of the U-shaped straight groove was 80 μm, and the spacing between two adjacent U-shaped straight grooves was 160 μm. The processed silicon carbide ceramic sample was placed in a beaker filled with anhydrous ethanol and ultrasonically cleaned for 30 minutes to obtain a silicon carbide ceramic substrate with a processed microstructure.

[0076] (2) Using a low-pressure plasma spraying method to prepare Yb on the microstructured silicon carbide ceramic substrate obtained in step (1) 2 Si 2 O 7 The process parameters of low-pressure plasma spraying are as follows: spraying distance 350 mm, current 650 A, hydrogen flow rate 12 L / min, substrate preheating temperature 600 °C; preparation of raw materials (Yb 2 Si 2 O 7 ) has a particle size range of 15-45 μm. The sprayed sample is air-cooled in a low-pressure plasma spraying device to obtain a deposited coating of silicon carbide ceramics.

[0077] Yb 2 Si 2 O 7 Due to the internal stress, longitudinal microcracks are successfully preformed at the raised positions between the microstructures inside the coating, and the crack width is 900nm-2μm.

[0078] Comparative Example 1

[0079] Comparative Example 1 uses traditional sandblasting to preform longitudinal cracks, and the specific method is as follows:

[0080] The silicon carbide ceramic sample was placed in a beaker filled with anhydrous ethanol and ultrasonically cleaned for 30 min. The surface of the sample was sandblasted with corundum grit at a pressure of 0.4 MPa. Then, the Yb 2 Si 2 O 7 Coating: The spraying distance is 1000 mm, the current is 2600 A, the argon flow rate is 110 L / min, and the substrate preheating temperature is 800° C. The particle size range of the prepared raw material is 15-45 μm, and silicon carbide ceramics with a deposited coating are obtained.

[0081] The cross section of the environmental barrier coating of Comparative Example 1 was observed by scanning electron microscopy, and the results are as follows: Figure 3 As shown. Figure 3 It can be seen that longitudinal cracks are obtained in the coating, with crack widths ranging from 800 nm to 3 μm.

[0082] Comparative Example 2

[0083] The only difference between Comparative Example 2 and Example 1 is that Comparative Example 2 uses an atmospheric plasma spraying method to deposit a coating on the surface of the substrate, and the rest is the same as Example 1.

[0084] A method for prefabricating longitudinal cracks in an environmental barrier coating comprises the following steps:

[0085] (1) The silicon carbide ceramic sample is placed in a beaker filled with anhydrous ethanol, ultrasonically cleaned for 30 minutes, and then placed in a special tooling filled with deionized water. The position of the silicon carbide sample is adjusted to maintain the water film thickness of 0.5 mm. A femtosecond laser is used to process the U-shaped straight groove structure on the surface of the silicon carbide ceramic. The process parameters are: laser power of 10 W, repetition frequency of 50 KHz, scanning speed of 1 mm / s, scanning times of 5 times, scanning spacing of 0.2 mm, defocusing amount of -1 mm, and processing environment of deionized water solution. The width of the processed U-shaped straight groove is 150 μm, the depth of the U-shaped straight groove is 80 μm, and the spacing between two adjacent U-shaped straight grooves is 160 μm; the processed silicon carbide ceramic sample is placed in a beaker filled with anhydrous ethanol and ultrasonically cleaned for 30 minutes to obtain a silicon carbide ceramic substrate with a processed microstructure;

[0086] (2) Using an atmospheric plasma spraying method to prepare Yb on the microstructured silicon carbide ceramic substrate obtained in step (1) 2 Si 2 O 7 The process parameters of plasma spray-physical vapor deposition are as follows: spray distance 130 mm, current 600 A, hydrogen flow rate 8 L / min, substrate preheating temperature 150 °C; preparation raw materials (Yb 2 Si 2 O 7) has a particle size range of 15-45 μm. The sample after spraying is air-cooled in an atmospheric environment to obtain a deposited coating of silicon carbide ceramics.

[0087] Due to atmospheric plasma spraying Yb 2 Si 2 O 7 There are many pores inside the coating, the coating density is insufficient, and regular longitudinal microcracks cannot be successfully prefabricated at the protruding positions of the microstructure.

[0088] Performance Testing

[0089] 1. Bonding strength test

[0090] The bonding strength between the coatings of Examples 1-6 and Comparative Examples 1-2 and the substrate was tested. The specific testing method of the bonding strength was carried out with reference to GB / T8642-2002.

[0091] The bonding strength results of the coating and the substrate in Examples 1-6 and Comparative Examples 1-2 are shown in Table 1.

[0092] Table 1: Bonding strength between coating and substrate of Examples 1-6 and Comparative Examples 1-2

[0093]

[0094] It can be seen from Table 1 that the coating and the substrate in the embodiment of the present invention have good bonding strength, which means that by processing the microstructure on the surface of the ceramic substrate and obtaining longitudinal cracks in the coating, the stress generated during the deposition of the coating can be released, thereby improving the bonding strength between the coating and the ceramic substrate and preventing the coating from peeling off during the spray deposition process.

[0095] Although longitudinal cracks were obtained in the coating by conventional sandblasting in Comparative Example 1, the bonding strength between the coating and the ceramic substrate was relatively small, which was significantly lower than the bonding strength between the coating and the ceramic substrate prepared by the present invention. The bonding strength between the coating and the ceramic substrate prepared by Example 4 of the present invention was 3.6 times that of Comparative Example 1.

[0096] Comparative Example 2 uses atmospheric plasma spraying to deposit the coating. Due to the difference in the deposition method, no longitudinal cracks are prefabricated in the coating in Comparative Example 2, and the bonding strength between the coating and the ceramic substrate is relatively small, which is significantly worse than the bonding strength between the coating and the ceramic substrate prepared in Example 1 of the present invention. This indicates that the use of a specific coating deposition method has an important influence on the bonding strength between the coating and the ceramic substrate.

[0097] 2. High temperature oxidation resistance

[0098] The coatings of Examples 1-6 and Comparative Examples 1-2 were tested for their high-temperature oxidation resistance. The specific test method is as follows: the ceramic samples of the deposited coatings prepared in Examples 1-6 and Comparative Examples 1-2 were placed in a constant temperature environment of 1400°C and maintained for a certain period of time to observe whether the coating peeled off. The high-temperature oxidation resistance of the coating was measured by whether the coating peeled off from the substrate after being maintained in a constant temperature environment of 1400°C for a certain period of time. If the coating peeled off from the ceramic substrate in a relatively short period of time, it means that the high-temperature oxidation resistance of the coating is poor. The longer the coating and the ceramic substrate maintain a good bonding state, the better the high-temperature oxidation resistance of the coating.

[0099] The high temperature oxidation resistance results of the coatings of Examples 1-6 and Comparative Examples 1-2 are shown in Table 2.

[0100] Table 2: High temperature oxidation resistance of coatings of Examples 1-6 and Comparative Examples 1-2

[0101]

[0102] It can be seen from Table 2 that the coatings with longitudinal cracks obtained in Examples 1-6 of the present invention are kept in a constant temperature environment of 1400°C for at least 150 hours without peeling off from the ceramic substrate, indicating that the coating has good bonding with the substrate, and further indicating that the coatings with longitudinal cracks prepared by the present invention have good resistance to high-temperature oxidation.

[0103] The coating obtained by conventional sandblasting in Comparative Example 1 fell off after being kept for 50 hours, indicating that the high temperature oxidation resistance of the coating in Comparative Example 1 is significantly worse than that of the coating prepared by the present invention, indicating that the present invention can not only improve the bonding strength between the coating and the ceramic substrate and avoid the coating from peeling off during the spray deposition process by processing the microstructure on the surface of the ceramic substrate, but also improve the high temperature oxidation resistance of the coating. In a high temperature environment, the coating and the ceramic substrate are still well bonded, and the coating is not easy to peel off from the ceramic substrate. Comparative Example 2 uses atmospheric plasma spraying to deposit the coating. Due to the difference in the deposition method, Comparative Example 2 does not prefabricate longitudinal cracks in the coating, and the bonding force between the coating and the ceramic substrate is small, so that the coating falls off from the substrate after being kept for 100 hours. The high temperature oxidation resistance of the coating in Comparative Example 2 is lower than that in Example 1.

[0104] 3. Thermal shock resistance

[0105] The purpose of the present invention to process microstructures on the surface of the ceramic substrate and then obtain longitudinal cracks in the coating is to release the stress generated during the deposition of the coating, improve the bonding strength between the coating and the ceramic substrate, and prevent the coating from peeling off during the spray deposition process. After obtaining a coating that is not easy to peel off, the coating containing longitudinal cracks may be penetrated into the coating through the longitudinal cracks during service by corrosive substances, causing the coating to fail prematurely. Therefore, the present invention adopts a high-temperature annealing method to promote the healing of the longitudinal cracks. The specific process is: the ceramic samples prepared in Examples 1-6 and Comparative Examples 1-2 are placed in a muffle furnace, the temperature is raised from room temperature to 1300°C, the heating rate is 5°C / min, and the temperature is kept for 10 hours.

[0106] After the ceramic sample prepared in Example 1 was treated as above, the cross section of the environmental barrier coating was observed by scanning electron microscopy. The results are as follows: Figure 4 As shown by Figure 4 It can be seen that the preformed longitudinal cracks in the coating are healed.

[0107] After treatment, the longitudinal cracks in the coatings of Examples 1-6 and Comparative Example 1 were all healed. Then, the thermal shock resistance test was performed on the samples prepared in Examples 1-6 and Comparative Example 1-2. The specific test method is as follows:

[0108] The samples of Examples 1-6 and Comparative Examples 1-2 were placed in a 1300°C furnace for 5±1min, taken out, and air-cooled for 5min, which was one cycle. The moisture on the coating surface should be blown off before the next thermal shock test. After the thermal shock test, the coating surface should be observed to have no warping, peeling, etc. The peeling of the coating along the four sides of the sample and within 3mm of the edge of the process hole is not counted. The test results show that the peeling area of ​​the coating of Examples 1-6 reached the failure standard (the peeling area is greater than 20% for failure) after 500, 520, 510, 550, 505, and 500 cycles respectively; the peeling area of ​​Comparative Examples 1-2 reached the failure standard (the peeling area is greater than 20% for failure) after 300 and 450 cycles respectively. It shows that the prefabricated coating of the present invention still has good thermal shock resistance after the longitudinal cracks are healed, and can well meet the later service requirements.

[0109] In summary, the present invention improves the bonding strength between the coating and the substrate by processing a microstructure of a specific shape on the surface of the substrate and combining a specific coating deposition method. The microstructure can adjust the internal stress of the coating, especially for high-density environmental barrier coatings. The coating deposited at the groove position generates compressive stress in the surface, and the protruding position generates tensile stress in the surface. The tensile and compressive stresses are mutually dependent, and prefabricated microcracks are formed at or near the protruding position of the microstructure, which can effectively release the stress generated during the coating deposition process, reduce the internal stress of the coating, increase the strain tolerance of the coating, and combine with a specific coating deposition method to improve the success rate of the deposited coating, thereby improving the bonding strength between the coating and the substrate and preventing the coating from falling off during the preparation process. The bonding strength between the coating with longitudinal cracks of the present invention and the substrate is significantly higher than the bonding strength between the coating and the substrate prepared by the traditional sandblasting roughening technology, which is 2.1-3.6 times that of the traditional sandblasting roughening technology. At the same time, after the longitudinal cracks are obtained, the longitudinal cracks can be healed by high-temperature annealing. After the cracks are healed, the coating still has good thermal vibration resistance, which can well meet the later service requirements.

[0110] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for prefabricating longitudinal cracks in an environmental barrier coating, characterized in that: The following steps are involved: The microstructure is machined on the substrate surface, and then the coating is deposited to form longitudinal cracks in the coating; The microstructure includes a plurality of U-shaped straight grooves, a plurality of V-shaped straight grooves or a plurality of U-shaped blind holes; The coating deposition method includes any one of plasma spraying-physical vapor deposition and low-pressure plasma spraying.

2. The prefabrication method according to claim 1, characterized in that: The matrix includes any one of silicon carbide ceramics, silicon carbide fiber reinforced silicon carbide ceramic matrix composite materials, and carbon fiber reinforced silicon carbide ceramic matrix composite materials.

3. The prefabrication method according to claim 1, characterized in that: A laser is used to process the surface of the substrate to form a microstructure.

4. The prefabrication method according to claim 1, characterized in that: The width of the U-shaped straight groove is 55 μm-330 μm, the depth of the U-shaped straight groove is 18 μm-220 μm, and the distance between two adjacent U-shaped straight grooves is 0 μm-550 μm.

5. The prefabrication method according to claim 1, characterized in that: The width of the V-shaped straight groove is 45 μm-550 μm, the depth of the V-shaped straight groove is 27 μm-330 μm, and the distance between two adjacent V-shaped straight grooves is 0 μm-550 μm.

6. The prefabrication method according to claim 1, characterized in that: The diameter of the U-shaped blind hole is 65 μm-880 μm, the depth of the U-shaped blind hole is 18 μm-330 μm, the spacing between two adjacent U-shaped blind holes in the X direction is 9 μm-550 μm; the spacing between two adjacent U-shaped blind holes in the Y direction is 9 μm-550 μm.

7. The prefabrication method according to claim 1, characterized in that: The composition of the coating includes any one of Re2Si2O7 and Re2SiO5; the Re includes any one of Yb, Y, Sc, Lu, and Er.

8. The prefabrication method according to claim 7, characterized in that: The coating has a thickness of 45-220 μm.

9. The prefabrication method according to any one of claims 1 to 8, characterized in that: The width of the longitudinal crack is 200nm-3.3μm.

10. An engine, characterized in that: It comprises a coating prepared by the method for prefabricating longitudinal cracks in an environmental barrier coating as described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Structure and method for improving bonding strength of wear-resistant anti-fatigue coating based on texture combined pattern

    CN107190227A

  • Thermal barrier coating provided with prefabricated microcosmic longitudinal crack structure and preparing method of thermal barrier coating

    CN108660407A

  • Novel thermal barrier coating structure and preparation method thereof

    CN113718188A

  • Laser micro-texture modified thermal barrier coating for delaying interface TGO growth and preparation process of laser micro-texture modified thermal barrier coating

    CN114807822A

  • Ceramic-based composite material with bionic multilevel structure and laser preparation method