Non-noble metal-biomass-based carbon material catalyst for hydrogen evolution by electrolyzing water as well as preparation method and application of non-noble metal-biomass-based carbon material catalyst

The non-precious metal-biomass-based carbon material catalyst treated by chitosan-phytic acid-Fe polymer and pore-forming agent solves the problem of poor performance of biomass carbon-based catalysts, and achieves efficient electrolysis of hydrogen and reduces the The potential and improve the catalytic performance.

CN118895522APending Publication Date: 2024-11-05QILU UNIVERSITY OF TECHNOLOGY (SHANDONG ACADEMY OF SCIENCES)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410923119.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing biomass carbon-based catalysts have poor catalytic performance during hydrolysis of hydrolysis, and their precious metal materials have limited resources and high costs, resulting in limited applications in the field of electrolytic water.

Method used

Chitosan-phytic acid-Fe polymer is used as the catalyst for non-precious metal-biomass-based carbon materials, and an efficient expansion flame retardant system is formed through electrostatic adsorption and phosphorus-nitrogen condensation reaction. Combined with pore-forming agent treatment, the specific surface area of ​​the catalyst is increased. and stability, reducing charge transfer resistance.

Benefits of technology

It significantly improves the stability and catalytic performance of the catalyst, reduces the overpotential during the electrolytic hydrogen analysis process, improves the wettability of the electrode-electrolyte interface, and achieves efficient hydrogen generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895522A_ABST
    Figure CN118895522A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electrocatalysts, in particular to a non-noble metal-biomass-based carbon material catalyst for hydrogen evolution by electrolyzing water as well as a preparation method and application of the non-noble metal-biomass-based carbon material catalyst. Dropwise adding a trivalent ferric salt solution into the chitosan acetic acid solution, and stirring for reaction; dropwise adding a phytic acid solution, and carrying out stirring reaction again; centrifugally collecting the precipitate, and washing the precipitate by using distilled water; freeze drying is carried out, such that a precursor catalyst is obtained; soaking the precursor of the catalyst in a pore-forming agent potassium hydroxide solution, and drying after ultrasonic treatment; after grinding, calcining to obtain the non-noble metal-biomass-based carbon material catalyst. The structure stability of the chitosan-phytic acid-Fe polymer in the carbonization process can improve the catalytic stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrocatalysts, and in particular to a non-precious metal-biomass-based carbon material catalyst for electrolyzing water to produce hydrogen, and a preparation method and application thereof. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] The increase in energy demand and the intensification of environmental pollution have prompted people to look for green and sustainable energy, including wind energy, tidal energy, and solar energy. However, a more effective method is needed to solve the defects of intermittent and localized new energy. Hydrogen is a promising alternative to fossil fuels that currently emit carbon dioxide due to its high calorific value, cleanliness, and recyclability. Producing hydrogen from renewable energy by electrolysis of water and using hydrogen-oxygen fuel cells to generate electricity can effectively solve the above problems and establish an energy system that meets the needs. The electrode reactions for electrocatalytic water splitting to produce hydrogen include the hydrogen evolution reaction (HER) occurring at the cathode and the oxygen evolution reaction (OER) occurring at the anode. In theory, the decomposition voltage of water electrolysis is only 1.23V. However, due to the existence of the reaction energy barrier, the working voltage required in the actual water electrolysis process is much higher than the theoretical value. To this end, it is necessary to develop high-performance water electrolysis catalysts to reduce the required overpotential.

[0004] Precious metal materials have been used in the field of water electrolysis due to their excellent catalytic activity. However, the limited reserves of precious metal natural resources, high cost and poor stability have restricted their widespread application. Therefore, it is very important to design non-precious metal hydrogen evolution catalysts with high activity, low cost and stable structure. At present, the application of biochar and its composite materials in electrocatalytic water splitting has been widely studied. Most biochar-based catalysts are prepared by doping metal ions into the biomass substrate through a simple process, and then depositing the metal on the surface of the substrate by carbonization. Due to the weak bond between biochar and metal ions, the metal ions will fall off; and the unstable biomass base framework and other factors make the catalytic performance of biochar material catalysts poor. Summary of the invention

[0005] In order to overcome the above problems, the present invention provides a non-precious metal-biomass-based carbon material catalyst for electrolysis of water for hydrogen evolution, and a preparation method and application thereof.

[0006] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:

[0007] The first aspect of the present invention provides a method for preparing a non-precious metal-biomass-based carbon material catalyst, comprising:

[0008] Add a trivalent iron salt solution to the chitosan acetic acid solution and stir to react; then add a phytic acid solution and stir to react again; collect the precipitate by centrifugation, wash the precipitate with distilled water; then freeze-dry to obtain a precursor catalyst;

[0009] The precursor catalyst is immersed in a pore-forming agent potassium hydroxide solution, and then dried after ultrasonic treatment; and then calcined after grinding to obtain a non-precious metal-biomass-based carbon material catalyst.

[0010] The second aspect of the present invention provides a non-precious metal-biomass-based carbon material catalyst prepared by the above preparation method.

[0011] The third aspect of the present invention provides the use of the above-mentioned non-precious metal-biomass-based carbon material catalyst in hydrogen evolution by water electrolysis.

[0012] The beneficial effects of the present invention are:

[0013] (1) In the present invention, Fe is first chelated by chitosan 3+ , and then the NH2 + There is electrostatic adsorption between the phosphate group on the phytic acid molecule and the phytic acid molecule and Fe 3+ There is also electrostatic adsorption, so with the help of the above-mentioned multiple forces, chitosan-phytic acid-Fe polymer is formed. At the same time, because chitosan and phytic acid have good flame retardant activity, the two will form a high-efficiency intumescent flame retardant system due to the phosphorus-nitrogen condensation carbonization reaction, which makes the chitosan-phytic acid-Fe polymer maintain a stable structure and not easy to collapse during high-temperature carbonization. The structural stability of the chitosan-phytic acid-Fe polymer during the carbonization process will improve the stability of the catalysis.

[0014] (2) In the present invention, the pore-forming agent enables the polymer to retain more pore structures after carbonization, thereby increasing the specific surface area of ​​the catalyst and thus improving the catalytic performance. At the same time, the rich heteroatom doping reduces the charge transfer resistance and improves the wettability of the electrode-electrolyte interface, thereby further improving the catalytic performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0016] Figure 1 The schematic diagram of the interaction principle of chitosan, phytic acid and Fe in the chitosan-phytic acid-Fe polymer prepared in the present invention;

[0017] Figure 2This is a scanning electron microscope image of the catalyst prepared in Example 6.

[0018] Figure 3 This is a transmission electron microscope image of the catalyst prepared in Example 6.

[0019] Figure 4 This is a graph showing the current variation over time for the catalyst prepared in Example 6. DETAILED DESCRIPTION

[0020] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0021] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0022] A first typical embodiment of the present invention provides a method for preparing a non-precious metal-biomass-based carbon material catalyst, comprising:

[0023] Add a trivalent iron salt solution to the chitosan acetic acid solution and stir to react; then add a phytic acid solution and stir to react again; collect the precipitate by centrifugation, wash the precipitate with distilled water; then freeze-dry to obtain a precursor catalyst;

[0024] The precursor catalyst is immersed in a pore-forming agent potassium hydroxide solution, and then dried after ultrasonic treatment; and then calcined after grinding to obtain a non-precious metal-biomass-based carbon material catalyst.

[0025] In one or more embodiments, the molecular weight of the chitosan is 40-60 kDa, preferably 50 kDa.

[0026] In one or more embodiments, the concentration of chitosan in the chitosan acetic acid solution is 4-6 g / L, preferably 5 g / L; the concentration of acetic acid is 0.05-0.2 M, preferably 0.1 M.

[0027] In one or more embodiments, the ferric iron salt includes one of FeCl3, Fe2(SO4)3, Fe(NO3)3 or Fe(CH3COO)3, preferably FeCl3.

[0028] In one or more embodiments, the concentration of the ferric iron salt solution is 0.05-0.2M, preferably 0.1M.

[0029] In one or more embodiments, the concentration of the phytic acid solution is 60-70 g / L, preferably 66 g / L.

[0030] In one or more embodiments, the volume ratio of the chitosan acetic acid solution to the trivalent iron salt solution and the phytic acid solution is 500:10-40:28-33, preferably 500:20:30.

[0031] In one or more embodiments, the precipitate is washed with distilled water until the pH of the precipitate is adjusted to 6.0-7.0.

[0032] In one or more embodiments, the concentration of the potassium hydroxide solution is 4 to 6 g / L, preferably 5 g / L.

[0033] In one or more embodiments, the mass ratio of potassium hydroxide to the catalyst precursor is 1:10 to 40, preferably 1:20.

[0034] In one or more embodiments, the calcination temperature is 400-900° C., preferably 600° C.; the calcination time is 1.5-3 h, preferably 2 h.

[0035] A second typical embodiment of the present invention provides a non-precious metal-biomass-based carbon material catalyst prepared by the above preparation method.

[0036] A third typical embodiment of the present invention provides the use of the above-mentioned non-precious metal-biomass-based carbon material catalyst in hydrogen evolution by electrolysis of water.

[0037] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.

[0038] In the following examples, a non-precious metal-biomass-based carbon material catalyst is loaded on nickel foam to form a cathode material for electrolyzing water to produce hydrogen. The specific preparation method includes:

[0039] Mix 0.25 mL of anhydrous ethanol with 0.25 mL of water, add 10 μL of Nafion solution and mix well to form a dispersant. Grind the catalysts prepared in the examples and comparative examples thoroughly, weigh 2 mg of the ground catalysts and disperse them in the above 0.5 mL of the dispersant. After ultrasonic treatment for 20 minutes, use a pipette to drop the dispersion into a 1×1 cm 2 To avoid sample loss, the dispersion should be added to the nickel foam several times, and then the sample should be dried at 60°C for 2 hours to form the cathode material for hydrogen production by water electrolysis.

[0040] In 1 M potassium hydroxide solution, the electrocatalytic water splitting hydrogen evolution effect of the catalysts obtained in the following examples and comparative examples was evaluated by a standard three-electrode system, and the calculated current density was 10 mA cm -2 The overpotential at .

[0041] Example 1

[0042] Chitosan with a molecular weight of 50kDa was completely dissolved in 0.1M glacial acetic acid solution to prepare a chitosan solution with a concentration of 5g / L. 20mL of FeCl3 solution (0.1M) was dripped dropwise into 500mL of chitosan acetic acid solution using a constant pressure funnel, and a magnetic stirrer was used to stir thoroughly during the process. 30mL of phytic acid solution (66g / L) was added to the mixed solution using a constant pressure funnel again, and stirring was continued until the solution was finished. The solution was centrifuged to collect the precipitate. The precipitate was washed several times with distilled water until the pH of the precipitate was adjusted to 6.0-7.0. The collected solid was freeze-dried to obtain the catalyst precursor.

[0043] Grind the precursor thoroughly, then put 300 mg of the ground precursor powder in a sample bottle, add 5 g / L potassium hydroxide solution, and make the mass ratio of precursor powder to potassium hydroxide 10:1. After ultrasonically treating the sample solution for 20 minutes, put the sample in a 60°C oven to dry. Grind the dried sample thoroughly, weigh it, and then transfer it to a corundum crucible. Set the tubular furnace program and carbonize it at 400°C for 2 hours to obtain a non-precious metal-biomass-based carbon material catalyst.

[0044] The non-precious metal-biomass-based carbon material catalyst obtained in this example was tested and its current density was 10 mA cm -2 The hydrogen evolution overpotential is 182.4 mV.

[0045] Example 2

[0046] Chitosan with a molecular weight of 50kDa was completely dissolved in 0.1M glacial acetic acid solution to prepare a chitosan solution with a concentration of 5g / L. 20mL of FeCl3 solution (0.1M) was dripped dropwise into 500mL of chitosan acetic acid solution using a constant pressure funnel, and a magnetic stirrer was used to stir thoroughly during the process. 30mL of phytic acid solution (66g / L) was added to the mixed solution using a constant pressure funnel again, and stirring was continued until the solution was finished. The solution was centrifuged to collect the precipitate. The precipitate was washed several times with distilled water until the pH of the precipitate was adjusted to 6.0-7.0. The collected solid was freeze-dried to obtain the catalyst precursor.

[0047] Grind the precursor thoroughly, then put 300 mg of the ground precursor powder in a sample bottle, add 5 g / L potassium hydroxide solution, and make the mass ratio of precursor powder to potassium hydroxide 20:1. After ultrasonically treating the sample solution for 20 minutes, put the sample into a 60°C oven for drying. Grind the dried sample thoroughly, weigh it, and then transfer it to a corundum crucible. Set the tubular furnace program and carbonize it at 400°C for 2 hours to obtain a non-precious metal-biomass-based carbon material catalyst.

[0048] The non-precious metal-biomass-based carbon material catalyst obtained in this example was tested and its current density was 10 mA cm -2 The hydrogen evolution overpotential is 216.2 mV.

[0049] Example 3

[0050] Chitosan with a molecular weight of 50kDa was completely dissolved in 0.1M glacial acetic acid solution to prepare a chitosan solution with a concentration of 5g / L. Use a constant pressure funnel to drop 20mL of FeCl3 solution (0.1M) into 500mL of chitosan acetic acid solution drop by drop, and use a magnetic stirrer to stir thoroughly during the process. Use a constant pressure funnel again to add 30mL of phytic acid solution (66g / L) to the above mixed solution, and continue stirring until it is finished. The solution was centrifuged to collect the precipitate. Wash the precipitate several times with distilled water until the pH of the precipitate is adjusted to 6.0-7.0. The collected solid was freeze-dried to obtain a precursor catalyst.

[0051] The precursor was fully ground, and then 300 mg of the ground precursor powder was placed in a sample bottle, and 5 g / L potassium hydroxide solution was added to make the mass ratio of the precursor powder to potassium hydroxide 40:1. After ultrasonic treatment of the sample solution for 20 minutes, the sample was placed in a 60°C oven for drying. The dried sample was fully ground and weighed, and then transferred to a corundum crucible. The tubular furnace program was set, and the non-precious metal-biomass-based carbon material catalyst was obtained by carbonization treatment at 400°C for 2 hours.

[0052] The non-precious metal-biomass-based carbon material catalyst obtained in this example was tested and its current density was 10 mA cm -2 The hydrogen evolution overpotential is 167.5 mV.

[0053] Example 4

[0054] Chitosan with a molecular weight of 50kDa was completely dissolved in 0.1M glacial acetic acid solution to prepare a chitosan solution with a concentration of 5g / L. 20mL of FeCl3 solution (0.1M) was dripped dropwise into 500mL of chitosan acetic acid solution using a constant pressure funnel, and a magnetic stirrer was used to stir thoroughly during the process. 30mL of phytic acid solution (66g / L) was added to the mixed solution using a constant pressure funnel again, and stirring was continued until the solution was finished. The solution was centrifuged to collect the precipitate. The precipitate was washed several times with distilled water until the pH of the precipitate was adjusted to 6.0-7.0. The collected solid was freeze-dried to obtain the catalyst precursor.

[0055] Grind the precursor thoroughly, then put 300 mg of the ground precursor powder in a sample bottle, add 5 g / L potassium hydroxide solution, and make the mass ratio of precursor powder to potassium hydroxide 10:1. After ultrasonically treating the sample solution for 20 minutes, put the sample into a 60°C oven for drying. Grind the dried sample thoroughly, weigh it, and then transfer it to a corundum crucible. Set the tubular furnace program and carbonize it at 900°C for 2 hours to obtain a non-precious metal-biomass-based carbon material catalyst.

[0056] The non-precious metal-biomass-based carbon material catalyst obtained in this example was tested and its current density was 10 mA cm -2 The hydrogen evolution overpotential is 214.8 mV.

[0057] Example 5

[0058] Chitosan with a molecular weight of 50kDa was completely dissolved in 0.1M glacial acetic acid solution to prepare a chitosan solution with a concentration of 5g / L. 20mL of FeCl3 solution (0.1M) was dripped dropwise into 500mL of chitosan acetic acid solution using a constant pressure funnel, and a magnetic stirrer was used to stir thoroughly during the process. 30mL of phytic acid solution (66g / L) was added to the mixed solution using a constant pressure funnel again, and stirring was continued until the solution was finished. The solution was centrifuged to collect the precipitate. The precipitate was washed several times with distilled water until the pH of the precipitate was adjusted to 6.0-7.0. The collected solid was freeze-dried to obtain the catalyst precursor.

[0059] Grind the precursor thoroughly, then put 300 mg of the ground precursor powder in a sample bottle, add 5 g / L potassium hydroxide solution, and make the mass ratio of precursor powder to potassium hydroxide 20:1. After ultrasonically treating the sample solution for 20 minutes, put the sample into a 60°C oven for drying. Grind the dried sample thoroughly, weigh it, and then transfer it to a corundum crucible. Set the tubular furnace program and carbonize it at 900°C for 2 hours to obtain a non-precious metal-biomass-based carbon material catalyst.

[0060] The non-precious metal-biomass-based carbon material catalyst obtained in this example was tested and its current density was 10 mA cm -2 The hydrogen evolution overpotential is 196.7 mV.

[0061] Example 6

[0062] Chitosan with a molecular weight of 50kDa was completely dissolved in 0.1M glacial acetic acid solution to prepare a chitosan solution with a concentration of 5g / L. 20mL of FeCl3 solution (0.1M) was dripped dropwise into 500mL of chitosan acetic acid solution using a constant pressure funnel, and a magnetic stirrer was used to stir thoroughly during the process. 30mL of phytic acid solution (66g / L) was added to the mixed solution using a constant pressure funnel again, and stirring was continued until the solution was finished. The solution was centrifuged to collect the precipitate. The precipitate was washed several times with distilled water until the pH of the precipitate was adjusted to 6.0-7.0. The collected solid was freeze-dried to obtain the catalyst precursor.

[0063] The precursor was fully ground, and then 300 mg of the ground precursor powder was placed in a sample bottle, and 5 g / L potassium hydroxide solution was added to make the mass ratio of the precursor powder to potassium hydroxide 20:1. After ultrasonic treatment of the sample solution for 20 minutes, the sample was placed in a 60°C oven for drying. After the dried sample was fully ground and weighed, it was transferred to a corundum crucible. The tubular furnace program was set up and carbonized at 600°C for 2 hours to obtain a non-precious metal-biomass-based carbon material catalyst.

[0064] The non-precious metal-biomass-based carbon material catalyst obtained in this example was tested and its current density was 10 mA cm -2 The hydrogen evolution overpotential is 139.4 mV.

[0065] Figure 4 The current density of the catalyst in this example is still basically maintained at -10mAcm after 108000s of testing. -2 , indicating that the sample has good stability

[0066] The microscopic morphology of the non-precious metal-biomass-based carbon material catalyst obtained in this example before and after carbonization is as follows: Figure 2 As shown, the CS-PA-Fe polymer is composed of countless spherical particles connected together, and its morphology does not change significantly after carbonization, which proves that during high-temperature carbonization, the CS-PA-Fe polymer can maintain a stable structure and is not easy to collapse.

[0067] The microstructure of the samples was further observed by transmission electron microscopy (TEM). Figure 3 After carbonization, metal deposition and aggregation occur and the lattice fringes are orderly, with a lattice spacing of 0.24 nm, corresponding to the (311) crystal plane of Fe3O4.

[0068] Comparative Example 1

[0069] The difference from Example 1 is that FeCl3 was not added during the catalyst preparation process, and only chitosan-phytic acid polymer was prepared. The optimal hydrogen evolution overpotential of the product under different conditions was 295mV, and the hydrogen evolution effect was poor compared with the chitosan-phytic acid-Fe polymer prepared in Example 1.

[0070] Comparative Example 2

[0071] The difference from Example 1 is that during the sample preparation process, Co(NO3)2·6H2O of the same concentration was used to replace FeCl3 to prepare chitosan-phytic acid-Co polymer. The optimal hydrogen evolution overpotential of the product under different conditions was 256 mV, and the hydrogen evolution effect was poorer than that of chitosan-phytic acid-Fe.

[0072] This is due to the interaction of chitosan and phytic acid with Fe 3+ It forms more metal coordination bonds and can firmly bind Fe 3+ .

[0073] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a non-precious metal-biomass-based carbon material catalyst, characterized in that: include: Add trivalent iron salt solution dropwise to the chitosan acetic acid solution and stir to react; Then, the phytic acid solution was added dropwise and the reaction was stirred again; Collect the precipitate by centrifugation, wash the precipitate with distilled water, and then freeze-dry to obtain a precursor catalyst; The precursor catalyst is immersed in a pore-forming agent potassium hydroxide solution, and then dried after ultrasonic treatment; After grinding, calcination is performed to obtain a non-precious metal-biomass-based carbon material catalyst.

2. The preparation method according to claim 1, characterized in that The molecular weight of the chitosan is 40-60 kDa, preferably 50 kDa; Alternatively, the chitosan concentration in the chitosan acetic acid solution is 4-6 g / L, preferably 5 g / L; the acetic acid concentration is 0.05-0.2 M, preferably 0.1 M.

3. The preparation method according to claim 1, characterized in that: The trivalent iron salt includes one of FeCl3, Fe2(SO4)3, Fe(NO3)3 or Fe(CH3COO)3, preferably FeCl3; Alternatively, the concentration of the ferric iron salt solution is 0.05-0.2M, preferably 0.1M.

4. The preparation method according to claim 1, characterized in that: The concentration of the phytic acid solution is 60-70 g / L, preferably 66 g / L.

5. The preparation method according to claim 1, characterized in that: The volume ratio of the chitosan acetic acid solution to the trivalent iron salt solution and the phytic acid solution is 500:10-40:28-33, preferably 500:20:

30.

6. The preparation method according to claim 1, characterized in that: The precipitate was washed with distilled water until the pH of the precipitate was adjusted to 6.0-7.

0.

7. The preparation method according to claim 1, characterized in that: The concentration of potassium hydroxide solution is 4-6 g / L, preferably 5 g / L; Alternatively, the mass ratio of potassium hydroxide to the precursor is 1:10 to 40, preferably 1:

20.

8. The preparation method according to claim 1, characterized in that: The calcination temperature is 400-900° C., preferably 600° C.; the calcination time is 1.5-3 h, preferably 2 h.

9. A non-precious metal-biomass-based carbon material catalyst prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the non-precious metal-biomass-based carbon material catalyst according to claim 9 in hydrogen evolution by water electrolysis.