Mxene composite Ni / Co nano-film prepared based on magnetron sputtering method, preparation method and application

The preparation of Mxene composite Ni/Co nanofilm by magnetron sputtering method solves the problem of high cost of precious metal catalysts, achieves low-cost and efficient electrocatalytic hydrogen evolution performance, and demonstrates good electrochemical stability and durability.

CN118895529APending Publication Date: 2024-11-05SOUTHWEST JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410924157.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

In the prior art, it is difficult to develop low-cost and high-efficiency non-precious metal HER catalysts due to high prices and scarcity, especially in the process of hydrogen production by water electrolysis, transition metals Fe, Co, Ni, oxides and sulfides. The application has not yet achieved ideal results.

Method used

Magnetic sputtering method was used to prepare Mxene composite Ni/Co nanofilm, and Ti3AlC2 precursor was etched by acid, magnetic stirring and sonication were performed to obtain a single layer of Mxene Ti3C2Tx solution, and after dropping on a carbon cloth, Ni and Co were used as The target was subjected to magnetron sputtering to prepare a Mxene composite Ni/Co nanofilm.

Benefits of technology

It significantly reduces the material cost, simplifies the preparation process, and achieves efficient electrocatalytic hydrogen evolution performance. The overpotential is only 141mV, and the potential remains basically unchanged at a current density of 10mA/cm2, with good stability and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895529A_ABST
    Figure CN118895529A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of electro-catalysis, and particularly relates to an Mxene composite Ni / Co nano-film prepared based on a magnetron sputtering method, a preparation method and application. The preparation method comprises the following steps: S1, carrying out acid etching on a Ti3AlC2 precursor, and carrying out magnetic stirring to obtain a mixture; washing and centrifuging the mixture, adjusting the pH value to obtain a precipitate, dispersing the precipitate in a solvent, adding LiCl, and stirring; performing centrifugation, extracting supernate after centrifugation, and performing ultrasonic treatment to obtain a single-layer Mxene Ti3C2Tx solution; and S2, dispensing a single-layer Mxene Ti3C2Tx solution on carbon cloth, heating and drying to obtain a Ti3C2Tx-loaded sample, adopting magnetron sputtering, adjusting parameters of magnetron sputtering, and preparing a Ni / Co nano-film on the sample by using a sputtering gun respectively with Ni and Co as targets to obtain the Mxene composite Ni / Co nano-film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electrocatalysis, and specifically relates to a Mxene composite Ni / Co nanofilm prepared based on a magnetron sputtering method, a preparation method and an application thereof. Background Art

[0002] Hydrogen production by water electrolysis is a promising technology for solving the energy crisis. Precious metals Pt, Ir, and Ag are the most effective electrocatalysts in reducing overpotential and accelerating HER kinetics. However, due to their high prices and scarcity, it is of great significance to develop low-cost, high-efficiency non-precious metal HER catalysts. Currently, transition metals Fe, Co, Ni and oxides and sulfides have been widely concerned by researchers in the field of hydrogen production by water electrolysis in the application of achieving low overpotential water decomposition. Therefore, the design efficiency of electrocatalysts can be improved by synthesizing them through simple process methods. It is urgent to provide a Mxene composite Ni / Co nanofilm prepared by magnetron sputtering, a preparation method and application. Summary of the invention

[0003] In view of the deficiencies in the prior art, the present invention provides a method for preparing a Mxene composite Ni / Co nanofilm based on a magnetron sputtering method, comprising the following steps:

[0004] S1: Acid-etching the Ti3AlC2 precursor and magnetically stirring to obtain a mixture; washing and centrifuging the mixture, adjusting the pH to obtain a precipitate, dispersing the precipitate in a solvent, adding LiCl and stirring; centrifuging, extracting the supernatant after centrifugation, and obtaining a single-layer Mxene Ti3C2T by ultrasonic treatment. x Solution;

[0005] S2: Monolayer Mxene Ti3C2T x The solution was dripped onto the carbon cloth and heated and dried to obtain the loaded Ti3C2T x The sample was prepared by magnetron sputtering and the parameters of magnetron sputtering were adjusted. Ni and Co were used as targets in the sputtering gun respectively to prepare Ni / Co nanofilm on the sample to obtain Mxene composite Ni / Co nanofilm.

[0006] Furthermore, the acid described in S1 includes hydrochloric acid and hydrofluoric acid.

[0007] Furthermore, the centrifugal speed described in S1 is 3500 rpm, and the centrifugal time is 1 minute.

[0008] Furthermore, the stirring time in S1 is 12 hours, and the stirring temperature is 35°C.

[0009] Furthermore, the ultrasonic time in S1 is 8 hours.

[0010] Furthermore, the heating temperature described in S2 is 60°C.

[0011] Furthermore, in the magnetron sputtering parameters described in S2, the substrate rotation speed is 2 rpm, and the initial vacuum degree is 9×10 -4 Pa, the sputtering gas is argon, the argon flow rate is 40 sccm, and the power of the DC sputtering source is 100 W.

[0012] A Mxene composite Ni / Co nanofilm prepared by magnetron sputtering.

[0013] The invention discloses an application of a Mxene composite Ni / Co nanofilm prepared by a magnetron sputtering method, wherein the Mxene composite Ni / Co nanofilm prepared by a magnetron sputtering method is applied in the preparation of a catalyst.

[0014] Technical Effects

[0015] (1) Advantages of nanofilms: The Mxene composite Ni / Co nanofilm prepared by magnetron sputtering provided by the present invention uses cheap metals Co and Ni as catalysts, which can significantly reduce material costs compared with precious metal catalysts.

[0016] (2) Advantages of the preparation method: The preparation method of the Mxene composite Ni / Co nanofilm based on magnetron sputtering provided by the present invention adopts physical magnetron sputtering preparation, and the preparation process uses physical deposition. Not only is the preparation process simple, but also it can achieve uniform, large-area preparation within a range of 4 inches, which plays a vital role in promoting the industrialization process; and the preparation time is greatly shortened, and the sample can be prepared in about 2 hours. At the same time, no by-products are generated and the pollution is small.

[0017] (3) Performance of nanofilm: The Mxene composite Ni / Co nanofilm prepared by magnetron sputtering provided by the present invention has good electrocatalytic hydrogen evolution performance as a catalyst, 10 mA / cm 2 The current density overpotential is only 141mV at 10mA / cm 2 The potential remains basically unchanged for 10 hours at a current density of . BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and should not be regarded as limiting the scope. For those of ordinary skill in the art, other relevant drawings can be obtained based on these drawings without creative work. In the drawings:

[0019] Figure 1 This is a schematic diagram of sample sputtering in Example 1 of the present invention;

[0020] Figure 2 Surface and cross-sectional views of the Mxene composite Ni / Co of Example 1 of the present invention;

[0021] Figure 3 The surface and cross-sectional view of Mxene composite Ni of Example 2 of the present invention;

[0022] Figure 4 Surface and cross-sectional views of Mxene composite Co of Example 3 of the present invention;

[0023] Figure 5 LSV curves of Pt sheets, Mxene composite Ni / Co, Mxene composite Ni, and Mxene composite Co in Examples 1 to 3 of the present invention;

[0024] Figure 6 The overpotential diagrams of Pt sheets, Mxene composite Ni / Co, Mxene composite Ni, and Mxene composite Co of Examples 1 to 3 of the present invention;

[0025] Figure 7 This is a stability test diagram of the present invention. DETAILED DESCRIPTION

[0026] The following will be combined with Examples 1 to 3 of the present invention and the attached Figures 1 to 7 , the technical solution of the present invention is clearly and completely described. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Combination Figure 1 The present invention provides a Mxene composite Ni / Co nanofilm prepared by magnetron sputtering, which specifically includes the following steps:

[0028] S1: First prepare Mxene Ti3C2T x solution, etching the Ti3AlC2 precursor with hydrochloric acid (HCl) and hydrofluoric acid (HF) solutions, slowly immersing the Ti3AlC2 MAX phase powder (300 mesh) in a mixture of hydrofluoric acid and hydrochloric acid under magnetic stirring, stirring continuously to obtain a mixture, then transferring the mixture to a centrifuge tube, washing with deionized water several times until the pH value of the supernatant is neutral, centrifuging is required for each washing, and in the last centrifugation cycle, a precipitate is obtained, the precipitate is dispersed in deionized water, and LiCl is added, stirred at room temperature, and then transferred to a centrifuge tube;

[0029] S2: Centrifuge the centrifuge tube of S1, remove the upper solution, resuspend the obtained precipitate in deionized water, ultrasonically centrifuge in an ice water bath, extract the supernatant, and collect the monolayer Ti3C2T x Ultrasonic treatment was performed to obtain a single-layer MxeneTi3C2T x Solution; cut the carbon cloth and place a single layer of Mxene Ti3C2T x The solution was evenly applied on the carbon cloth using a needle tube. About 10 drops were then dried on a heating table at 60 °C to obtain the loaded Ti3C2T x The sample was then magnetron sputtered. Two adjacent sputtering guns were used in the sputtering chamber. The center line of the three targets was an equilateral triangle, slightly close and inclined at about 15°. One sputtering gun sputtered with a Co (purity of 99.9%) target, and the other sputtering gun sputtered with a Ni (purity of 99.9%) target. The Ti3C2T x The carbon cloth was used as the substrate, the rotation speed of the substrate was set, and before starting the sputtering, the sputtering chamber was first evacuated using a mechanical pump and a molecular pump, and then the sputtering gas argon (purity of 99.999%) was introduced into the sputtering chamber, and the two DC sputtering sources were controlled to 100W, and the Co target and the Ni target were synchronously magnetron sputtered to obtain the Mxene composite Ni / Co nanofilm.

[0030] Example 1

[0031] S1: 2 g of Ti3AlC2 MAX phase powder (300 mesh) was slowly immersed in a mixture of 20 mL 49% HF and 20 mL 12 M HCl under magnetic stirring. The solution was stirred continuously at 35 °C for 12 h to obtain a mixture, which was then transferred to a centrifuge tube and washed several times with deionized water until the pH of the supernatant was neutral. Each washing step required centrifugation at a rate of 3500 rpm for 1 min. In the last centrifugation, the prepared precipitate was dispersed in 40 mL deionized water and 2 g LiCl was added. Stir at room temperature for 12 h and then transferred to a centrifuge tube;

[0032] S2: Centrifuge the tube at 3500 rpm for 1 minute and remove the upper solution. Resuspend the resulting precipitate in deionized water, sonicate in an ice water bath for 15 minutes, and centrifuge at 3000 rpm for 15 minutes. After extracting the supernatant, the collected monolayer Ti3C2T x The single-layer Mxene Ti3C2T was obtained by ultrasonic treatment for 8 h. x Solution; cut the carbon cloth into 3.3×1cm 2 , then MxeneTi3C2T xThe solution was evenly applied on the carbon cloth using a needle, and then dried on a heating table at 60 °C to obtain a Ti3C2T x The sample was then prepared by magnetron sputtering. In the sputtering chamber, two adjacent sputtering guns were used to make the center line of the three targets form an equilateral triangle, slightly close to each other and tilted about 15°. One sputtering gun sputtered with a Co (purity of 99.9%) target, and the other sputtering gun sputtered with a Ni (purity of 99.9%) target; the Ti3C2T x The carbon cloth was used as the substrate, and the substrate speed was set to 2 r / min. Before starting the sputtering, the sputtering chamber was evacuated using a mechanical pump and a molecular pump. -4 Pa, argon gas (purity of 99.999%) was introduced into the sputtering chamber with a flow rate of 40 sccm to make the vacuum degree reach 2Pa, and the two DC sputtering sources were controlled to be 100W. The Co target and the Ni target were synchronously magnetron sputtered for 7 minutes and 8 seconds to obtain the Mxene composite Ni / Co nanofilm, and the thickness of the Ni / Co nanofilm was 223.9nm.

[0033] Combination Figure 2 SEM images of the surface and cross section of the Mxene composite Ni / Co nanofilm can be obtained.

[0034] Example 2

[0035] S1: 2 g of Ti3AlC2 MAX phase powder (300 mesh) was slowly immersed in a mixture of 20 mL 49% HF and 20 mL 12 M HCl under magnetic stirring. The solution was stirred continuously at 35 °C for 12 h to obtain a mixture, which was then transferred to a centrifuge tube and washed several times with deionized water until the pH of the supernatant was neutral. Each washing step required centrifugation at a rate of 3500 rpm for 1 min. In the last centrifugation, the prepared precipitate was dispersed in 40 mL deionized water and 2 g LiCl was added. Stir at room temperature for 12 h and then transferred to a centrifuge tube;

[0036] S2: Centrifuge the tube at 3500 rpm for 1 minute and remove the upper solution. Resuspend the resulting precipitate in deionized water, sonicate in an ice water bath for 15 minutes, and centrifuge at 3000 rpm for 15 minutes. After extracting the supernatant, the collected monolayer Ti3C2T x The single-layer Mxene Ti3C2T was obtained by ultrasonic treatment for 8 h. x Solution; cut the carbon cloth into 3.3×1cm 2 , then MxeneTi3C2T xThe solution was evenly applied on the carbon cloth using a needle, and then dried on a heating table at 60 °C to obtain a Ti3C2T x The sample was then prepared by magnetron sputtering. In the sputtering chamber, only one sputtering gun was used to deposit Ni, so that the center line of the three targets was an equilateral triangle, slightly close to the tilt of about 15°. In the sputtering chamber, the sputtering gun sputtered with Ni (purity of 99.9%) target; with Ti3C2T x The carbon cloth was used as the substrate, and the substrate speed was set to 2 r / min. Before starting the sputtering, the sputtering chamber was evacuated using a mechanical pump and a molecular pump. -4 Pa, argon gas (purity of 99.999%) was introduced into the sputtering chamber, the argon flow rate was 40sccm, the vacuum degree reached 2Pa, the DC sputtering source was 100W, and the Ni target was magnetron sputtered for 14 minutes; the Mxene composite Ni nanofilm was obtained, and the thickness of the Ni nanofilm was 281.9nm.

[0037] Combination Figure 3 SEM images of the surface and cross section of the Mxene composite Ni nanofilm in Example 2 can be obtained.

[0038] Example 3

[0039] S1: 2 g of Ti3AlC2 MAX phase powder (300 mesh) was slowly immersed in a mixture of 20 mL 49% HF and 20 mL 12 M HCl under magnetic stirring. The solution was stirred continuously at 35 °C for 12 h to obtain a mixture, which was then transferred to a centrifuge tube and washed several times with deionized water until the pH of the supernatant was neutral. Each washing step required centrifugation at a rate of 3500 rpm for 1 min. In the last centrifugation, the prepared precipitate was dispersed in 40 mL deionized water and 2 g LiCl was added. Stir at room temperature for 12 h and then transferred to a centrifuge tube;

[0040] S2: Centrifuge the tube at 3500 rpm for 1 minute and remove the upper solution. Resuspend the resulting precipitate in deionized water, sonicate in an ice water bath for 15 minutes, and centrifuge at 3000 rpm for 15 minutes. After extracting the supernatant, the collected monolayer Ti3C2T x The single-layer Mxene Ti3C2T was obtained by ultrasonic treatment for 8 h. x Solution; cut the carbon cloth into 3.3×1cm 2 , then MxeneTi3C2T x The solution was evenly applied on the carbon cloth using a needle, and then dried on a heating table at 60 °C to obtain a Ti3C2T xThe sample was then prepared by magnetron sputtering. In the sputtering chamber, only one sputtering gun was used to deposit Co. The center line of the three targets was made into an equilateral triangle, slightly close to the tilt of about 15°. In the sputtering chamber, the sputtering gun sputtered with a Co (purity of 99.9%) target; the target was loaded with Ti3C2T x The carbon cloth was used as the substrate, and the substrate speed was set to 2 r / min. Before starting the sputtering, the sputtering chamber was evacuated using a mechanical pump and a molecular pump. -4 Pa, argon gas (purity of 99.999%) was introduced into the sputtering chamber, the argon flow rate was 40sccm, the vacuum degree reached 2Pa, the two DC sputtering sources were controlled to 100W, and the Co target was magnetron sputtered for 15 minutes; the Mxene composite Co nanofilm was obtained, and the thickness of the Co nanofilm was 209.1nm.

[0041] Combination Figure 4 The surface and cross-sectional SEM images of the Mxene composite Co nanofilm can be obtained; combined with Figure 5 The electrocatalytic measurements were performed in a three-electrode configuration with Ag / AgCl as the reference electrode. A carbon rod was used as the counter electrode and the Mxene composite Ni / Co was used as the working electrode. The linear sweep voltammetry (LSV) curve was measured with 1 mol / L KOH as the electrolyte. The LSV scan rate was 10 mVs -1 . At the same time, the loading of single-layer Co, single-layer Ni and 1×1cm 2 The electrocatalytic performance of the Pt sheet, combined with Figure 6 By comparing the overpotential of MXene composite Ni / Co, we can see that the overpotential of MXene composite Ni / Co can reach 141mV. Figure 7 , Figure 7 The prepared Mxene composite Ni / Co is at 10mA / cm 2 After 10 hours of long-term durability test at a current density of 2.5 Å, it can be seen from the figure that the potential change of the electrode is negligible, indicating good stability.

[0042] The present invention provides a Mxene composite Ni / Co nanofilm prepared by magnetron sputtering, which uses low-cost metal Co and Ni as catalysts. Compared with commonly used traditional precious metals, it significantly reduces material costs and improves economic benefits; by adopting physical magnetron sputtering technology, a simple and fast preparation process is achieved. The method utilizes the principle of physical deposition, avoids complex chemical reactions and the generation of by-products, and reduces environmental pollution; and the preparation process time is greatly shortened, and the sample preparation can be completed in only about 2 hours, which improves production efficiency.

[0043] The present invention provides a Mxene composite Ni / Co nanofilm prepared by magnetron sputtering, which, as a catalyst, exhibits good electrocatalytic hydrogen evolution performance. 2 At a current density of , the overpotential is only 141 mV. In addition, during a long period of electrocatalysis (such as 10 hours), the potential remains basically stable, indicating that the nanofilm has excellent electrochemical stability and durability. The present invention not only has significant advantages in cost, preparation process and environmental friendliness, but also exhibits excellent performance in electrocatalytic performance and has broad application prospects.

Claims

1. A method for preparing a Mxene composite Ni / Co nanofilm based on magnetron sputtering, characterized in that: The following steps are involved: S1: A Ti3AlC2 precursor is acid-etched and magnetically stirred to obtain a mixture; the mixture is washed and centrifuged, the pH is adjusted to obtain a precipitate, the precipitate is dispersed in a solvent, LiCl is added and stirred; centrifugation is performed, the supernatant after centrifugation is extracted, and a single-layer Mxene Ti3C2T is obtained by ultrasonic treatment. x Solution; S2: Monolayer Mxene Ti3C2T x The solution was dripped onto the carbon cloth and heated and dried to obtain the loaded Ti3C2T x The sample was prepared by magnetron sputtering and the parameters of magnetron sputtering were adjusted. Ni and Co were used as targets in the sputtering gun respectively to prepare Ni / Co nanofilm on the sample to obtain Mxene composite Ni / Co nanofilm.

2. The method for preparing a Mxene composite Ni / Co nanofilm based on magnetron sputtering according to claim 1, characterized in that: The acid described in S1 includes hydrochloric acid and hydrofluoric acid.

3. The method for preparing a Mxene composite Ni / Co nanofilm based on magnetron sputtering according to claim 1, characterized in that: The centrifugation speed described in S1 was 3500 rpm and the centrifugation time was 1 minute.

4. The method for preparing a Mxene composite Ni / Co nanofilm based on magnetron sputtering according to claim 1, characterized in that: The stirring time in S1 was 12 hours, and the stirring temperature was 35°C.

5. The method for preparing a Mxene composite Ni / Co nanofilm based on magnetron sputtering according to claim 1, characterized in that: The ultrasonic time described in S1 was 8 hours.

6. The method for preparing a Mxene composite Ni / Co nanofilm based on magnetron sputtering according to claim 1, characterized in that: The heating temperature described in S2 is 60°C.

7. The method for preparing a Mxene composite Ni / Co nanofilm based on magnetron sputtering according to claim 1, characterized in that: The magnetron sputtering parameters described in S2 include a substrate rotation speed of 2 rpm and an initial vacuum degree of 9×10 -4 Pa, the sputtering gas is argon, the argon flow rate is 40 sccm, and the power of the DC sputtering source is 100 W.

8. A Mxene composite Ni / Co nanofilm prepared by magnetron sputtering method according to any one of the preparation methods of claims 1 to 7.

9. The use of a Mxene composite Ni / Co nanofilm prepared by magnetron sputtering according to claim 8, characterized in that: The Mxene composite Ni / Co nanofilm prepared based on the magnetron sputtering method is used in the preparation of catalysts.