Oxygen evolution catalyst as well as preparation method and application thereof

By using CeO2 core-loaded IrO2 particles with a large specific surface area in the oxygen evolution catalyst, the core-shell structure is formed, which solves the problem of agglomeration of iridium oxide of precious metals, improves the durability and dispersion of the catalyst, reduces the amount of Ir, and achieves efficient Oxygen evolution catalytic effect.

CN118895534APending Publication Date: 2024-11-05山东国创燃料电池技术创新中心有限公司
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410941756.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-05

Smart Images

  • Figure CN118895534A_ABST
    Figure CN118895534A_ABST
Patent Text Reader

Abstract

The invention provides an oxygen evolution catalyst as well as a preparation method and application thereof. The oxygen evolution catalyst comprises a CeO2 core and IrO2 particles loaded outside the CeO2 core. According to the oxygen evolution catalyst, a CeO2 core with a large specific surface area and a rough surface is used as a carrier, IrO2 particles are loaded on the surface of the carrier in situ, and a core-shell structure with iridium oxide nanoparticles wrapped outside the CeO2 core is formed; the large specific surface area of the CeO2 core in the oxygen evolution catalyst can provide favorable attachment sites for IrO2 particles, and the core-shell structure with CeO2 as the core and IrO2 as the shell can effectively improve the dispersity of IrO2, facilitates exposure of active sites and reduces the dosage of Ir; besides, a synergistic effect exists between the CeO2 core and metal in the IrO2 particles, a confinement effect is achieved on the IrO2 particles, migration and agglomeration of IrO2 can be effectively avoided, the structural stability is improved, and therefore the durability of the oxygen evolution catalyst is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of catalysts and relates to an oxygen evolution catalyst, in particular to an oxygen evolution catalyst and a preparation method and application thereof. Background Art

[0002] Iridium oxide catalyst is a key component of the catalyst layer of proton exchange membrane water electrolysis, which is used to catalyze the oxygen evolution reaction. However, the precious metal iridium oxide is expensive and scarce, and it is easy to agglomerate during the synthesis process and long-term durability. Therefore, it is very important to improve the utilization rate of precious metals and improve their durability.

[0003] CN111375408A discloses a preparation method and application of an iridium oxide nanoparticle catalyst to solve the problem that iridium oxide is prone to agglomeration and forming large particles during the synthesis process. The invention uniformly coats a mixed solution containing a polymer and an iridium-containing compound on a treated conductive substrate, then calcines in an air atmosphere to convert the iridium-containing compound into iridium oxide while decomposing the polymer, thereby obtaining an iridium oxide nanoparticle material with a small particle size, amorphous and porous structure, and uses a plasma generator to remove the polymer remaining on the iridium oxide nanoparticle material, so that the surface of the iridium oxide nanoparticle is rich in hydroxyl groups. The invention uses a film formed by the polymer in the mixed solution to solve the problem of agglomeration and forming large particles when the iridium-containing compound is calcined to generate iridium oxide nanoparticles, thereby obtaining iridium oxide nanoparticles with small particle size. Finally, a plasma generator is used to remove the polymer remaining during the calcination process, increase the contact area of ​​the iridium oxide nanoparticles, and thus improve the catalytic efficiency of the iridium oxide nanoparticles. However, the decomposition of the polymer and the conversion of the iridium-containing compound may not occur simultaneously. If the polymer is completely decomposed before the iridium-containing compound is converted, it will not play the role of a template, and the iridium-containing compound will inevitably agglomerate during the conversion process of iridium oxide.

[0004] CN114645295A discloses a method for preparing an anode catalyst for electrolysis of water, wherein a solution formed by iridium-containing salt, alkali metal nitrate, alkali metal acetate and semi-light amine hydrochloride is mixed with a salt solution containing niobium to form a sol system, and then immediately frozen with liquid nitrogen to obtain a light yellow precursor powder, which is then calcined at high temperature and centrifuged and washed. The composite catalyst of iridium oxide prepared by the inventive method forms a three-dimensional structure of twisted and wound nanosheets, and the catalyst has a higher specific surface area, which can effectively improve the utilization rate of iridium; at the same time, since niobium doping improves the conductivity of the catalyst and provides skeleton support for iridium oxide, the iridium oxide catalyst can still maintain its structure at high potential, thereby effectively improving the service life and corrosion resistance of the catalyst. However, the speed of liquid nitrogen freezing used in the patent is not controllable, so the crystallization speed of each substance is different, and it is difficult to stably form a wrapping structure with iridium as the core, and during the calcination process, the metal salt will melt, exposing the iridium wrapped inside, and the iridium will also migrate and agglomerate in the metal salt in the molten state, thereby forming a large-sized iridium oxide.

[0005] CN108486615A discloses a method for preparing a hydrometallurgical iridium-cerium-zirconium ternary composite oxide anode, which belongs to the field of hydrometallurgy. The prepared anode is composed of a titanium substrate and an oxide coating, in which the iridium dioxide is in the rutile phase, the zirconium dioxide is in the amorphous phase, and the cerium dioxide is in the fluorite phase, which is different from the traditional Ti / IrO 2 Compared with the anode, the addition of zirconium promotes the oxygen evolution active substance IrO 2 The addition of cerium during the precipitation of crystals has the effect of refining the grains, effectively increasing the oxygen evolution active surface area of ​​the anode. The invention has a simple preparation process, and the anode obtained has good oxygen evolution catalytic activity and service life. In addition, since the precious metal elements in the coating are replaced by zirconium and cerium, the production cost of the anode is effectively reduced, and it is a hydrometallurgical anode with great prospects for use. However, the anode prepared by the preparation method of the hydrometallurgical iridium-cerium-zirconium ternary composite oxide anode has the problem of easy agglomeration during long-term durability.

[0006] The currently disclosed oxygen evolution catalysts have certain defects. There is a problem of high cost due to the high content of precious metal iridium oxide, and the problem of poor stability due to easy agglomeration during the synthesis process and long-term use. Therefore, it is very important to develop and design a new type of oxygen evolution catalyst and its preparation method. Summary of the invention

[0007] In view of the shortcomings of the prior art, the present invention aims to provide an oxygen evolution catalyst and a preparation method and application thereof. The oxygen evolution catalyst provided by the present invention is CeO with a large specific surface area and a rough surface. 2 The core is the carrier, and the surface of the carrier is in situ loaded with IrO 2particles, forming CeO 2 The core-shell structure of iridium oxide nanoparticles wrapped outside the core; CeO 2 The large specific surface area of ​​the core can be IrO 2 The particles provide favorable attachment sites to CeO 2 As the core, IrO 2 The core-shell structure of IrO 2 The dispersion of CeO is helpful to expose the active sites and reduce the amount of Ir. 2 Core and IrO 2 There is a synergistic effect between the metals in the particles, which has a great influence on the IrO 2 The particles play a confining role and can effectively avoid IrO 2 Migration and agglomeration increase the structural stability, thereby enhancing the durability of the oxygen evolution catalyst.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides an oxygen evolution catalyst, the oxygen evolution catalyst comprising CeO 2 core, and the CeO 2 IrO externally loaded on the core 2 Particles.

[0010] The oxygen evolution catalyst provided in the present invention is CeO with large specific surface area and rough surface. 2 The core is the carrier, and the surface of the carrier is in situ loaded with IrO 2 particles, forming CeO 2 The core-shell structure of iridium oxide nanoparticles wrapped outside the core; CeO 2 The large specific surface area of ​​the core can be IrO 2 The particles provide favorable attachment sites to CeO 2 As the core, IrO 2 The core-shell structure of IrO 2 The dispersion of CeO is helpful to expose the active sites and reduce the amount of Ir. 2 Core and IrO 2 There is a synergistic effect between the metals in the particles, which has a great influence on the IrO 2 The particles play a confining role and can effectively avoid IrO 2 Migration and agglomeration increase the structural stability, thereby enhancing the durability of the oxygen evolution catalyst.

[0011] Preferably, the CeO 2The average particle size of the core is 150 to 250 nm, for example, it can be 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, 200 nm, 210 nm, 220 nm, 230 nm, 240 nm or 250 nm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0012] Preferably, the CeO 2 The particle size range of the core is 1 to 30 nm, for example, it can be 1 nm, 3 nm, 5 nm, 7 nm, 10 nm, 12 nm, 15 nm, 17 nm, 20 nm, 22 nm, 25 nm, 27 nm or 30 nm, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0013] The particle size range of the present invention is CeO 2 The difference between the maximum and minimum particle sizes of the core.

[0014] Preferably, the IrO 2 The particle size range of the particles is 1 to 10 nm, for example, 1 nm, 3 nm, 5 nm, 7 nm, 9 nm or 10 nm, but is not limited to the listed values. Other unlisted values ​​within the numerical range are also applicable, preferably 2 to 5 nm.

[0015] Preferably, the CeO 2 The shape of the nucleus is spherical.

[0016] In a second aspect, the present invention provides a method for preparing the oxygen evolution catalyst according to the first aspect, the preparation method comprising:

[0017] (1) The Ce source solution is subjected to hydrothermal treatment to obtain a solid, and the obtained solid is subjected to heat treatment in an oxidizing atmosphere to obtain CeO 2 nuclear;

[0018] (2) The CeO obtained in step (1) 2 The core, the alkaline solution and the Ir source solution are mixed to obtain a mixed solution, the mixed solution is subjected to hydrothermal treatment to obtain a solid, and the solid is subjected to heat treatment in an oxidizing atmosphere to obtain the oxygen evolution catalyst.

[0019] The oxidizing atmosphere in step (1) and step (2) of the preparation method of the present invention comprises an air atmosphere.

[0020] Preferably, the Ce source in the Ce source solution in step (1) comprises Ce(NO 3 ) 3 6H 2 O、CeCl 3 or Ce2 (SO 4 ) 3 ·4H 2 O, any one or a combination of at least two, a typical but non-limiting combination includes Ce(NO 3 ) 3 6H 2 O and CeCl 3 Combination of CeCl 3 With Ce 2 (SO 4 ) 3 ·4H 2 O combination, or Ce(NO 3 ) 3 6H 2 O、CeCl 3 With Ce 2 (SO 4 ) 3 ·4H 2 O combination.

[0021] Preferably, the solvent in the Ce source solution in step (1) includes any one of ammonia water, sodium hydroxide solution or ethylene glycol, or a combination of at least two of them. Typical but non-limiting combinations include a combination of ammonia water and sodium hydroxide solution, a combination of sodium hydroxide solution and ethylene glycol, or a combination of ammonia water, sodium hydroxide solution and ethylene glycol.

[0022] Preferably, the Ce source solution in step (1) also includes a dispersant, and the dispersant includes any one of polyvinyl pyrrolidone, sodium dodecyl sulfonate or sodium p-aminobenzenesulfonate, or a combination of at least two of them. Typical but non-limiting combinations include a combination of polyvinyl pyrrolidone and sodium dodecyl sulfonate, a combination of sodium dodecyl sulfonate and sodium p-aminobenzenesulfonate, or a combination of polyvinyl pyrrolidone, sodium dodecyl sulfonate and sodium p-aminobenzenesulfonate.

[0023] Preferably, the mass ratio of the Ce source to the dispersant in the Ce source solution in step (1) is (1-20):1, for example, it can be 1:1, 3:1, 5:1, 7:1, 10:1, 12:1, 14:1, 16:1, 18:1 or 20:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0024] Preferably, the concentration of the Ce source in the Ce source solution in step (1) is 10 to 50 mg / mL, for example, 10 mg / mL, 15 mg / mL, 20 mg / mL, 25 mg / mL, 30 mg / mL, 35 mg / mL, 40 mg / mL, 45 mg / mL or 50 mg / mL, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0025] Preferably, the hydrothermal treatment in step (1) is carried out in a high-pressure reactor at a temperature of 80 to 200° C. for 6 to 20 hours.

[0026] The temperature of the hydrothermal treatment in the present invention is 80-200°C, for example, it can be 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C or 200°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] Preferably, the hydrothermal treatment and the heat treatment in step (1) further include solid-liquid separation, washing and drying performed sequentially.

[0028] Preferably, the solid-liquid separation comprises centrifugal separation.

[0029] Preferably, the washing comprises washing three times with deionized water and ethanol in a mixing ratio of 1:1.

[0030] Preferably, the drying temperature is 50-70° C. and the drying time is 10-14 hours.

[0031] The drying temperature in the present invention includes 50-70°C, for example, it can be 50°C, 52°C, 54°C, 56°C, 58°C, 60°C, 62°C, 64°C, 66°C, 68°C or 70°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0032] The drying time in the present invention is 10 to 14 hours, for example, it can be 10 hours, 10.5 hours, 11 hours, 11.5 hours, 12 hours, 12.5 hours, 13 hours, 13.5 hours or 14 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] Preferably, the heat treatment in step (1) is performed at a temperature of 500 to 800° C. and for a time of 5 to 10 hours.

[0034] The temperature of the heat treatment in step (1) of the present invention is 500-800°C, for example, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C or 800°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] The heat treatment time in step (1) of the present invention is 5 to 10 hours, for example, 5 hours, 5.5 hours, 6 hours, 6.5 hours, 7 hours, 7.5 hours, 8 hours, 8.5 hours, 9 hours, 9.5 hours or 10 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0036] Preferably, in step (2), the CeO obtained in step (1) is mixed 2 The mass ratio of the core to the alkaline solution is (1-4):1, for example, it can be 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1 or 4:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] Preferably, in step (2), the CeO obtained in step (1) is mixed 2 The mass ratio of the core to the Ir source solution is (1-5):1, for example, 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1 or 5:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] Preferably, the alkaline solution in step (2) comprises NaOH solution, KOH solution or NH 3 ·H 2 O solution, a typical but non-limiting combination includes a combination of a NaOH solution and a KOH solution, a KOH solution and a NH 3 ·H 2 O, or NaOH solution, KOH solution and NH 3 ·H 2 O solution combination.

[0039] Preferably, the concentration of the alkaline solution in step (2) is 0.05-0.15 mol / L, for example, it can be 0.05 mol / L, 0.06 mol / L, 0.07 mol / L, 0.08 mol / L, 0.09 mol / L, 0.1 mol / L, 0.11 mol / L, 0.12 mol / L, 0.13 mol / L, 0.14 mol / L or 0.15 mol / L, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0040] Preferably, the Ir source in the Ir source solution in step (2) comprises H 2 IrCl 6 、IrCl 3 or Ir 2 S 3Any one or a combination of at least two of the following, typical but non-limiting combinations include H 2 IrCl 6 With IrCl 3 Combination of IrCl 3 With Ir 2 S 3 A combination of, or H 2 IrCl 6 、IrCl 3 With Ir 2 S 3 combination.

[0041] Preferably, the concentration of the Ir source in the Ir source solution in step (2) is 5 to 20 mg / mL, for example, 5 mg / mL, 7 mg / mL, 9 mg / mL, 10 mg / mL, 12 mg / mL, 14 mg / mL, 16 mg / mL, 18 mg / mL or 20 mg / mL, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0042] Preferably, the mixing method in step (2) includes ultrasound for 20 to 40 minutes, for example, it can be 20 minutes, 22 minutes, 24 minutes, 26 minutes, 28 minutes, 30 minutes, 32 minutes, 34 minutes, 36 minutes, 38 minutes or 40 minutes, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0043] Preferably, the temperature of the hydrothermal treatment in step (2) is 100-200° C. and the time is 15-30 hours.

[0044] The temperature of the hydrothermal treatment in step (2) of the present invention is 100-200°C, for example, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C or 200°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0045] Preferably, the hydrothermal treatment and the heat treatment in step (2) also include solid-liquid separation, washing and drying performed sequentially.

[0046] Preferably, the solid-liquid separation comprises centrifugal separation.

[0047] Preferably, the washing comprises washing three times with deionized water and ethanol in a mixing ratio of 1:1.

[0048] Preferably, the drying temperature is 50-70° C. and the drying time is 10-14 hours.

[0049] The drying temperature in the present invention is 50-70°C, for example, it can be 50°C, 52°C, 54°C, 56°C, 58°C, 60°C, 62°C, 64°C, 66°C, 68°C or 70°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0050] The drying time in the present invention is 10 to 14 hours, for example, it can be 10 hours, 10.5 hours, 11 hours, 11.5 hours, 12 hours, 12.5 hours, 13 hours, 13.5 hours or 14 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0051] Preferably, the heat treatment in step (2) is carried out at a temperature of 200 to 600° C. and for a time of 3 to 9 hours.

[0052] The temperature of the heat treatment in step (2) of the present invention is 200-600°C, for example, it can be 200°C, 250°C, 300°C, 350°C, 400°C, 450°C, 500°C, 550°C or 600°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0053] The heat treatment time in step (2) of the present invention is 3 to 9 hours, for example, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, 5.5 hours, 6 hours, 6.5 hours or 7 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0054] As a preferred technical solution of the preparation method of the present invention, the preparation method comprises:

[0055] (1) A Ce source solution containing a dispersant at a concentration of 10 to 50 mg / mL is subjected to a hydrothermal treatment at 80 to 200° C. for 6 to 20 hours to obtain a solid, and the obtained solid is subjected to a heat treatment at 500 to 800° C. for 5 to 10 hours in an oxidizing atmosphere to obtain CeO 2 nuclear;

[0056] (2) The CeO obtained in step (1) with a mass ratio of (1-4):1 2 The CeO 2 The mass ratio of the core to the alkaline solution is (1-4):1, the CeO 2 The mass ratio of the core to the Ir source solution is (1-5):1; the obtained mixed solution is hydrothermally treated at 100-200°C for 15-30h to obtain a solid, and the obtained solid is heat-treated at 200-600°C for 3-9h in an oxidizing atmosphere to obtain the oxygen evolution catalyst.

[0057] In a third aspect, the present invention provides an application of the oxygen evolution catalyst described in the first aspect, wherein the oxygen evolution catalyst is used for electrolyzing water to evolve oxygen.

[0058] Compared with the prior art, the present invention has the following beneficial effects:

[0059] The oxygen evolution catalyst provided in the present invention is CeO with large specific surface area and rough surface. 2 The core is the carrier, and the surface of the carrier is in situ loaded with IrO 2 particles, forming CeO 2 The core-shell structure of iridium oxide nanoparticles wrapped outside the core; CeO 2 The large specific surface area of ​​the core can be IrO 2 The particles provide favorable attachment sites to CeO 2 As the core, IrO 2 The core-shell structure of IrO 2 The dispersion of CeO is helpful to expose the active sites and reduce the amount of Ir. 2 Core and IrO 2 There is a synergistic effect between the metals in the particles, which has a great influence on the IrO 2 The particles play a confining role and can effectively avoid IrO 2 Migration and agglomeration increase the structural stability, thereby enhancing the durability of the oxygen evolution catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] Figure 1 This is the SEM image of the oxygen evolution catalyst in Example 1.

[0061] Figure 2 This is the energy spectrum of the oxygen evolution catalyst in Example 1.

[0062] Figure 3 Element distribution diagram of the oxygen evolution catalyst in Example 1.

[0063] Figure 4 This is the TEM image of the oxygen evolution catalyst in Example 1.

[0064] Figure 5 1 is a test curve of polarization performance of a single cell prepared with the oxygen evolution catalyst in Example 1 and Comparative Example 1.

[0065] Figure 6 The polarization performance test curves of the single cells prepared with the oxygen evolution catalysts in Example 1 and Comparative Example 1 after 100 hours of endurance. DETAILED DESCRIPTION

[0066] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0067] Example 1

[0068] This embodiment provides an oxygen evolution catalyst, which includes spherical CeO with an average particle size of 200 nm and a particle size range of 15 nm. 2 core, and the CeO 2 The particle size of IrO loaded on the core is in the range of 2 to 5 nm. 2 Particles;

[0069] The preparation method of the oxygen evolution catalyst is:

[0070] (1) Ce(NO) containing polyvinyl pyrrolidone dispersant at a concentration of 20 mg / mL 3 ) 3 6H 2 O solution was hydrothermally treated at 140 °C for 13 h to obtain a solid, which was then heat treated at 650 °C for 8 h in an oxidizing atmosphere to obtain CeO 2 nuclear;

[0071] (2) The CeO obtained in step (1) 2 Nucleus, 0.1 mol / L NaOH solution and 10 mg / mL H 2 IrCl 6 The solutions are mixed to obtain a mixed solution, wherein the CeO 2 The mass ratio of the core to the NaOH solution is 2:1. 2 Nucleus and H 2 IrCl 6 The mass ratio of the solution is 3:1. The obtained mixed solution is subjected to hydrothermal treatment at 150° C. for 25 hours to obtain a solid. The obtained solid is heat-treated at 400° C. for 6 hours in an oxidizing atmosphere to obtain the oxygen evolution catalyst.

[0072] Example 2

[0073] This embodiment provides an oxygen evolution catalyst, which includes spherical CeO with an average particle size of 150 nm and a particle size range of 18 nm. 2 core, and the CeO 2 The particle size of IrO loaded on the core is in the range of 1 to 4 nm. 2 Particles;

[0074] The preparation method of the oxygen evolution catalyst is:

[0075] (1) Ce(NO) containing polyvinyl pyrrolidone dispersant at a concentration of 30 mg / mL 3 ) 3 6H 2 The O solution was hydrothermally treated at 80 °C for 20 h to obtain a solid, which was then heat treated at 500 °C for 10 h in an oxidizing atmosphere to obtain CeO 2 nuclear;

[0076] (2) The CeO obtained in step (1) 2 Nucleus, NaOH solution with a concentration of 0.15 mol / L and H 2 IrCl 6 The solutions are mixed to obtain a mixed solution, wherein the CeO 2 The mass ratio of the core to the NaOH solution is 1:1. 2 Nucleus and H 2 IrCl 6 The mass ratio of the solution is 4:1; the obtained mixed solution is subjected to hydrothermal treatment at 100° C. for 30 hours to obtain a solid, and the obtained solid is subjected to heat treatment at 200° C. for 9 hours in an oxidizing atmosphere to obtain the oxygen evolution catalyst.

[0077] Example 3

[0078] This embodiment provides an oxygen evolution catalyst, which includes spherical CeO with an average particle size of 250 nm and a particle size range of 30 nm. 2 core, and the CeO 2 The particle size of the core external load is 6-10nm IrO 2 Particles;

[0079] The preparation method of the oxygen evolution catalyst is:

[0080] (1) Ce(NO) containing polyvinyl pyrrolidone dispersant at a concentration of 15 mg / mL 3 ) 3 6H 2 O solution was hydrothermally treated at 200 °C for 6 h to obtain a solid, which was then heat treated at 800 °C for 5 h in an oxidizing atmosphere to obtain CeO 2 nuclear;

[0081] (2) The CeO obtained in step (1) 2 Nucleus, NaOH solution with a concentration of 0.05 mol / L and H 2 IrCl 6 The solutions are mixed to obtain a mixed solution, wherein the CeO 2 The mass ratio of the core to the NaOH solution is 1:1.2 Nucleus and H 2 IrCl 6 The mass ratio of the solution is 2:1; the obtained mixed solution is subjected to hydrothermal treatment at 200° C. for 15 hours to obtain a solid, and the obtained solid is subjected to heat treatment at 600° C. for 3 hours in an oxidizing atmosphere to obtain the oxygen evolution catalyst.

[0082] Example 4

[0083] This embodiment provides an oxygen evolution catalyst, except that the spherical CeO 2 The average particle size of the core is 120 nm and the particle size range is 20 nm. The step (1) of the preparation method is: Ce(NO 3 ) 3 6H 2 The O solution was hydrothermally treated at 120 °C for 16 h to obtain a solid, which was then heat treated at 600 °C for 4 h in an oxidizing atmosphere to obtain CeO 2 Except for the core, the rest is the same as in Example 1.

[0084] Example 5

[0085] This embodiment provides an oxygen evolution catalyst, except that the spherical CeO 2 The average particle size of the core is 300 nm and the particle size range is 26 nm. The step (1) of the preparation method is: Ce(NO 3 ) 3 6H 2 The O solution was hydrothermally treated at 150 °C for 15 h to obtain a solid, which was then heat treated at 500 °C for 5 h in an oxidizing atmosphere to obtain CeO 2 Except for the core, the rest is the same as in Example 1.

[0086] Example 6

[0087] This embodiment provides an oxygen evolution catalyst, except that IrO 2 The particle size range of the particles is 0.1 to 0.7 nm. The step (2) in the preparation method is: CeO obtained in step (1) 2 Nucleus, NaOH solution with a concentration of 0.05 mol / L and H 2 IrCl 6 The solutions are mixed to obtain a mixed solution, wherein the CeO 2 The mass ratio of the core to the NaOH solution is 4:1. 2 Nucleus and H 2IrCl 6 The mass ratio of the solution is 5:1; the obtained mixed solution is subjected to hydrothermal treatment at 130°C for 13 hours to obtain a solid, and the obtained solid is heat-treated at 500°C for 3 hours in an oxidizing atmosphere to obtain the oxygen evolution catalyst, and the rest is the same as Example 1.

[0088] Example 7

[0089] This embodiment provides an oxygen evolution catalyst, except that IrO 2 The particle size range of the particles is 14 to 20 nm. The step (2) in the preparation method is: CeO obtained in step (1) 2 Nucleus, 0.1 mol / L NaOH solution and 10 mg / mL H 2 IrCl 6 The solutions are mixed to obtain a mixed solution, wherein the CeO 2 The mass ratio of the core to the NaOH solution is 1:1. 2 Nucleus and H 2 IrCl 6 The mass ratio of the solutions is 1:1; the obtained mixed solution is subjected to hydrothermal treatment at 140°C for 16 hours to obtain a solid, and the obtained solid is heat-treated at 600°C for 5 hours in an oxidizing atmosphere to obtain the oxygen evolution catalyst, and the rest is the same as Example 1.

[0090] Example 8

[0091] This embodiment provides an oxygen evolution catalyst, which includes spherical CeO with an average particle size of 300 nm and a particle size range of 350 nm and a smooth surface. 2 core, and the CeO 2 The core is loaded with IrO particles with a particle size range of 30-80 nm. 2 Particles.

[0092] The preparation method of the oxygen evolution catalyst is:

[0093] (1) Ce(NO) containing polyvinyl pyrrolidone dispersant at a concentration of 30 mg / mL 3 ) 3 6H 2 The O solution was fully mixed with a urea solution with a concentration of 60 mg / mL, citric acid was added to make its content 1.5 g / L, and a solid was obtained after hydrothermal treatment at 120°C for 8 h. The obtained solid was heat treated at 500°C for 10 h in an oxidizing atmosphere to obtain CeO 2 nuclear;

[0094] (2) The CeO obtained in step (1) 2Nucleus, NaOH solution with a concentration of 0.15 mol / L and H 2 IrCl 6 The solutions are mixed to obtain a mixed solution, wherein the CeO 2 The mass ratio of the core to the NaOH solution is 1:1. 2 Nucleus and H 2 IrCl 6 The mass ratio of the solution is 4:1; the obtained mixed solution is subjected to hydrothermal treatment at 100° C. for 30 hours to obtain a solid, and the obtained solid is subjected to heat treatment at 200° C. for 9 hours in an oxidizing atmosphere to obtain the oxygen evolution catalyst.

[0095] Comparative Example 1

[0096] This comparative example provides an oxygen evolution catalyst, wherein the oxygen evolution catalyst comprises IrO 2 catalyst;

[0097] The preparation method of the oxygen evolution catalyst is:

[0098] A 0.15 mol / L NaOH solution and a 5 mg / mL H 2 IrCl 6 The solutions are mixed to obtain a mixed solution, the mixed solution is subjected to a hydrothermal treatment at 100° C. for 30 hours to obtain a solid, and the solid is subjected to a heat treatment at 200° C. for 9 hours in an oxidizing atmosphere to obtain the oxygen evolution catalyst.

[0099] The oxygen evolution catalyst provided in Example 1 was scanned using a scanning electron microscope to obtain a SEM image of the oxygen evolution catalyst in Example 1. Figure 1 shown; from Figure 1 It can be seen that CeO in the oxygen evolution catalyst prepared in the embodiment 2 The core is uniformly distributed nanospheres, and CeO 2 The surface of the core is slightly rough, which can provide more specific surface area for the loading of active components, thereby increasing the reaction active sites; the oxygen evolution catalyst provided in Example 1 was tested using EDS energy spectrum, and the energy spectrum of the oxygen evolution catalyst was obtained as shown in Figure 2 shown; from Figure 2 It can be seen that the element composition of the oxygen evolution catalyst provided in Example 1 is mainly Ce and O, and also contains a small amount of C; the element distribution diagram of the oxygen evolution catalyst provided in Example 1 obtained by scanning with a scanning electron microscope is as follows: Figure 3 As shown by Figure 3 It can be seen that the elements of the oxygen evolution catalyst provided in Example 1 are evenly distributed;

[0100] The oxygen evolution catalyst provided in Example 1 was scanned using a transmission electron microscope to obtain a TEM image of the oxygen evolution catalyst in Example 1. Figure 4 shown by Figure 4 Available, IrO 2 The particles are uniformly loaded on the spherical CeO 2 The surface of the core forms a stable core-shell structure, IrO 2 The size is very small, only about 2-5nm, achieving small-size and highly dispersed IrO 2 The preparation of Ir greatly reduces the amount of precious metal Ir and improves the atomic utilization rate.

[0101] The oxygen evolution catalysts provided in the above embodiments and comparative examples were compared for single cell performance; first, a single cell was prepared, and the slurry formula used was as follows: the oxygen evolution catalysts provided in the above embodiments and comparative examples were respectively taken and dispersed in a mixed solution of water and isopropanol, wherein the alcohol-water ratio was 3:1, and then a certain amount of membrane solution was added to the mixed solution so that the slurry I / C was 0.5, and the two were placed in a cell crusher for 60 minutes of cell crushing for standby use, and the mixed catalyst slurry was sprayed on the surface of the proton exchange membrane using an acoustic sprayer to obtain a membrane electrode, and then a single cell was prepared from a single cell; wherein the Ir loading on the membrane electrode prepared with the oxygen evolution catalyst in Example 1 was less than 1 mg cm -2 The Ir loading on the membrane electrode prepared with the oxygen evolution catalyst in Example 8 was 1.1 mg cm -2 The Ir loading on the membrane electrode prepared with the oxygen evolution catalyst in Comparative Example 1 was 1.5 mg cm -2 .

[0102] The polarization performance test of the obtained single cell was carried out under the following conditions: at a test temperature of 80°C, the test results showed that the single cell had a polarization performance of 1A / cm 2 The decomposition voltage under current density is shown in Table 1, wherein the single cell polarization performance test curves of the oxygen evolution catalysts provided in Example 1 and Comparative Example 1 are shown in Figure 5 As shown;

[0103] The obtained single cell was used to carry out oxygen evolution catalytic reaction for 100 h, and then the single cell was subjected to durability test. The conditions of the single cell durability test were: at a test temperature of 80 ° C, at 1 A / cm 2 The battery was operated at a current density of 100 h for 100 h, and the test showed that the battery had a durability of 100 h at 1 A / cm 2The decomposition voltage under the current density is calculated, and the performance attenuation of the single cell is calculated as shown in Table 1. The calculation formula of the performance attenuation is: performance attenuation (%) = decomposition voltage increment / initial decomposition voltage × 100%; wherein, the single cell polarization performance test curve of the oxygen evolution catalyst provided in Example 1 and Comparative Example 1 after 100h durability is as shown in Figure 6 shown.

[0104] Table 1

[0105]

[0106] From Table 1, we can get:

[0107] (1) The single cell prepared with the oxygen evolution catalyst provided in Examples 1 to 3 of the present invention was subjected to an 2 It has a lower oxygen evolution decomposition voltage under current density, and the performance attenuation after 100h endurance is small;

[0108] (2) By comparing Example 1 with Examples 4 and 5, it can be seen that the spherical CeO 2 The average particle size of the core will affect the performance of the single cell prepared with the oxygen evolution catalyst; when the spherical CeO 2 If the average particle size of the core is too small, the impedance of the single cell will increase. 2 The decomposition voltage under current density becomes higher, and the performance decay after 100h durability becomes larger. This is due to the CeO 2 When the core particle size is too small, due to CeO 2 The close contact between particles increases the mass transfer resistance, thus increasing the impedance and decreasing the performance. 2 When the average particle size of the core is too large, the impedance of the single cell will decrease. 2 The decomposition voltage under current density becomes higher, and the performance decay after 100h durability becomes larger. This is due to the CeO 2 The core particle size is too large, the specific surface area is reduced, and it is not enough to load IrO 2 , leading to IrO 2 Agglomeration occurs, the exposed effective active area is reduced, and the performance is reduced;

[0109] (3) By comparing Example 1 with Examples 6 and 7, it can be seen that the IrO in the oxygen evolution catalyst provided by the present invention 2 The particle size range of the particles will affect the performance of the single cell prepared with the oxygen evolution catalyst; when the IrO 2 When the particle size range is too small, the impedance of the single battery will increase. 2 The decomposition voltage under current density becomes higher, and the performance degradation after 100h durability becomes larger. This is due to the IrO2 If the particles are too small, the contact between the particles will not be close enough, the charge transfer resistance will increase, and the performance will decrease. 2 When the particle size range is too large, the impedance of the single battery will decrease. 2 The decomposition voltage under current density becomes higher, and the performance degradation after 100h durability becomes larger. This is due to the IrO 2 If the particles are too large, the effective active surface will be reduced, the metal utilization rate will decrease, and the performance will be reduced;

[0110] (4) By comparing Example 1 with Example 8, it can be seen that the oxygen evolution catalyst provided in the present invention is CeO with uniform particle size, large specific surface area and rough surface. 2 The core is the carrier, and the surface of the carrier is in situ loaded with IrO 2 particles, forming CeO 2 The core-shell structure of iridium oxide nanoparticles wrapped outside the core; CeO 2 The large specific surface area and abundant surface defects of the core can provide a promising target for IrO 2 The particles provide favorable attachment sites, increasing the IrO 2 The dispersion of CeO particles can avoid the migration and agglomeration of metal particles, which is helpful for the exposure of active sites, thereby reducing the size and loading of Ir. 2 Nanospheres loaded with IrO 2 The core-shell structure formed is more stable, and IrO 2 The particle size is also more uniform, which is of great significance for improving the durability of membrane electrodes;

[0111] (4) By comparing Example 1 with Comparative Example 1, it can be seen that compared with the simple IrO 2 The single cell prepared by the catalyst, the single cell prepared by the oxygen evolution catalyst provided in this application at 1A / cm 2 The decomposition voltage under current density becomes smaller, and the performance decay after 100h durability becomes smaller. This is due to the spherical CeO 2 The core is important for increasing IrO 2 The dispersion of particles plays an important role in increasing the effective active area of ​​oxygen evolution catalysts, and CeO 2 The addition of can effectively increase the durability of the oxygen evolution catalyst, and the metal-metal interaction increases the stability of the core-shell structure.

[0112] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. An oxygen evolution catalyst, characterized in that The oxygen evolution catalyst comprises a CeO2 core and IrO2 particles loaded outside the CeO2 core.

2. The oxygen evolution catalyst according to claim 1, characterized in that The average particle size of the CeO2 core is 150 to 250 nm; Preferably, the particle size range of the CeO2 core is 1 to 30 nm; Preferably, the particle size of the IrO2 particles is in the range of 1 to 10 nm, preferably 2 to 5 nm.

3. The oxygen evolution catalyst according to claim 1 or 2, characterized in that The CeO2 core is spherical in shape.

4. A method for preparing the oxygen evolution catalyst according to any one of claims 1 to 3, characterized in that: The preparation method comprises: (1) subjecting a Ce source solution to hydrothermal treatment to obtain a solid, and subjecting the obtained solid to heat treatment in an oxidizing atmosphere to obtain a CeO2 core; (2) The CeO2 core obtained in step (1), the alkaline solution and the Ir source solution are mixed to obtain a mixed solution, the obtained mixed solution is subjected to hydrothermal treatment to obtain a solid, and the obtained solid is subjected to heat treatment in an oxidizing atmosphere to obtain the oxygen evolution catalyst.

5. The preparation method according to claim 4, characterized in that: The Ce source in the Ce source solution of step (1) includes any one of Ce(NO3)3·6H2O, CeCl3 or Ce2(SO4)3·4H2O or a combination of at least two thereof; Preferably, the solvent in the Ce source solution in step (1) comprises any one of ammonia water, sodium hydroxide solution or ethylene glycol, or a combination of at least two thereof; Preferably, the Ce source solution in step (1) further comprises a dispersant, and the dispersant comprises any one of polyvinyl pyrrolidone, sodium dodecyl sulfate or sodium p-aminobenzenesulfonate, or a combination of at least two thereof; Preferably, the concentration of the Ce source in the Ce source solution in step (1) is 10 to 50 mg / mL.

6. The preparation method according to claim 4 or 5, characterized in that: The hydrothermal treatment in step (1) is carried out in a high pressure reactor at a temperature of 80 to 200° C. for a period of 6 to 20 hours; Preferably, the heat treatment in step (1) is performed at a temperature of 500 to 800° C. and for a time of 5 to 10 hours.

7. The preparation method according to any one of claims 4 to 6, characterized in that: In the mixing of step (2), the mass ratio of the CeO2 core obtained in step (1) to the alkaline solution is (1-4):1; Preferably, in the mixing of step (2), the mass ratio of the CeO2 core obtained in step (1) to the Ir source solution is (1-5):1; Preferably, the concentration of the alkaline solution in step (2) is 0.05 to 0.15 mol / L; Preferably, the Ir source in the Ir source solution in step (2) comprises any one of H2IrCl6, IrCl3 or Ir2S3, or a combination of at least two thereof; Preferably, the concentration of the Ir source in the Ir source solution in step (2) is 5 to 20 mg / mL.

8. The preparation method according to any one of claims 4 to 7, characterized in that: The temperature of the hydrothermal treatment in step (2) is 100 to 200° C. and the time is 15 to 30 hours; Preferably, the heat treatment in step (2) is carried out at a temperature of 200 to 600° C. and for a time of 3 to 9 hours.

9. The preparation method according to any one of claims 4 to 8, characterized in that: The preparation method comprises: (1) subjecting a Ce source solution containing a dispersant at a concentration of 10 to 50 mg / mL to a hydrothermal treatment at 80 to 200° C. for 6 to 20 hours to obtain a solid, and subjecting the obtained solid to a heat treatment at 500 to 800° C. for 5 to 10 hours in an oxidizing atmosphere to obtain a CeO2 core; (2) The CeO2 core obtained in step (1), an alkaline solution with a concentration of 0.05-0.15 mol / L and an Ir source solution with a concentration of 5-20 mg / mL are mixed to obtain a mixed solution, wherein the mass ratio of the CeO2 core to the alkaline solution is (1-4):1, and the mass ratio of the CeO2 core to the Ir source solution is (1-5):1; the obtained mixed solution is subjected to hydrothermal treatment at 100-200°C for 15-30h to obtain a solid, and the obtained solid is subjected to heat treatment at 200-600°C for 3-9h in an oxidizing atmosphere to obtain the oxygen evolution catalyst.

10. An application of the oxygen evolution catalyst according to claim 1, characterized in that: The oxygen evolution catalyst is used for electrolyzing water to evolve oxygen.

Citation Information

Patent Citations

  • Preparation method of iridium cerium zirconium ternary composite oxide inert anode

    CN108486615A

  • Preparation method and application of iridium oxide nanoparticle catalyst

    CN111375408A

  • Preparation method of anode catalyst for electrolyzing water

    CN114645295A