Low-resistance composite substrate structure and preparation method

The 3C SiC single crystal support layer was manufactured by the liquid phase method and formed a low resistance composite substrate structure, which solved the problems of low manufacturing efficiency and high resistivity of existing silicon carbide single crystal substrates, and achieved low resistivity and high yield rate power device manufacturing.

CN118895564APending Publication Date: 2024-11-05TJ INNOVATIVE SEMICON SUBSTRATE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410964458.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing manufacturing methods of silicon carbide single crystal substrates are inefficient and costly, and have a large resistivity of the support substrate, which affects the vertical on-resistance and performance of the power devices.

Method used

The 3C SiC single crystal support layer was manufactured by liquid phase method. By mixing and heating raw materials in a graphite crucible, crystal growth was performed using a high-pressure nitrogen environment, supporting layer with a resistivity less than 1 mΩ·cm was prepared, and the ion implantation and film layer were used. Transfer to form a low resistance composite substrate structure.

Benefits of technology

It significantly reduces the manufacturing cycle and cost of power devices, reduces or eliminates the back thinning steps, and improves the yield and resistivity performance of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895564A_ABST
    Figure CN118895564A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of semiconductor material preparation, in particular to a low-resistance composite substrate structure and a preparation method. A low-resistance composite substrate structure comprises a supporting layer and a film layer formed on the supporting layer. The film layer is single crystal silicon carbide, and the crystal form is a 4H type; the supporting layer is single crystal silicon carbide, and the crystal form is 3C type; and the resistivity of the supporting layer is less than 1m omega.cm. According to the composite substrate, the resistivity of the supporting substrate is very low, the back thinning amount is greatly reduced, even the back thinning step is not needed, the manufacturing period and cost of a power device are greatly reduced, and the yield of the device is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of semiconductor material preparation, and in particular to a low-resistance composite substrate structure and a preparation method thereof. Background Art

[0002] Devices made of silicon carbide single crystal substrates have the advantages of high temperature resistance, high voltage resistance, high frequency, high power, radiation resistance, and high efficiency. They have important application value in radio frequency, new energy vehicles and other fields.

[0003] The conventional manufacturing method of silicon carbide single crystal substrate includes the following process: growing silicon carbide single crystal by physical vapor transport method to obtain a silicon carbide single crystal ingot; processing the periphery of the ingot to obtain the required diameter and surface quality, then slicing the ingot into thin slices, grinding and polishing the slices to the required thickness and flatness, and obtaining the final silicon carbide single crystal substrate. The efficiency of growing silicon carbide single crystal by physical vapor transport method is very low, resulting in high cost of single silicon carbide single crystal substrate. One solution to reduce the cost of silicon carbide substrate is to use a composite substrate structure: forming a single crystal silicon carbide thin layer on a lower-priced silicon carbide substrate.

[0004] The resistivity of the support substrate is a key parameter. The resistivity of the support substrate is relatively large. After manufacturing power devices on a thin layer of silicon carbide single crystal, the surface (i.e., the back side) of the support substrate needs to be thinned to reduce the vertical on-resistance of the device. The surface treatment quality of the bonding surface between the support substrate and the donor substrate must also be considered. The surface treatment quality of the bonding surface directly affects the quality of the composite substrate, thereby affecting the device performance.

[0005] Therefore, it is necessary to propose a supporting substrate with low resistivity and high bonding quality to manufacture power devices with low vertical on-resistance. Summary of the invention

[0006] The purpose of the present invention is to provide a low-resistance composite substrate structure and manufacturing method, wherein the supporting substrate is a 3C-type SiC single crystal, manufactured by a liquid phase method, and has a resistivity of <1mΩ·cm, meeting the industry's low resistivity requirements. With the composite substrate of the present invention, since the resistivity of the supporting substrate is very low, the back thinning amount is greatly reduced, and even the back thinning step may not be required, which greatly reduces the manufacturing cycle and cost of power devices and improves the device yield.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] A low-resistance composite substrate structure comprises a support layer and a film layer formed on the support layer;

[0009] The film layer is single crystal silicon carbide, and the crystal form is 4H type; it can also be 6H crystal form or 3C crystal form;

[0010] The support layer is single crystal silicon carbide, and the crystal form is 3C type;

[0011] The resistivity of the support layer is less than 1 mΩ·cm.

[0012] Furthermore, the nitrogen doping concentration of the support layer is 1.5-2.5E20atom / cm 3 .

[0013] Furthermore, the support layer is prepared by a liquid phase method, and the preparation relies on a preparation device, and the preparation device includes a furnace body;

[0014] A graphite crucible for containing raw materials is provided in the furnace body;

[0015] A seed crystal rod is provided above the graphite crucible;

[0016] A seed crystal holder is arranged at one end of the seed crystal rod, and a silicon carbide seed crystal is arranged on the seed crystal holder;

[0017] A heating device, used to provide the temperature required for preparation;

[0018] The atmosphere device is used to provide the atmosphere environment required for preparation.

[0019] Furthermore, the preparation method of the support layer includes:

[0020] a. Loading: Mix the raw materials evenly and put them in a graphite crucible;

[0021] b. Chemical material: heating the raw materials to melt them and form alloy solution;

[0022] c. Growth: ascending and rotating the seed crystal rod to pull and grow the crystal to obtain the crystal;

[0023] d. Prepare the support layer: cut, thin, grind and polish the crystal to obtain the support layer.

[0024] Furthermore, after step a, it also includes atmosphere preparation;

[0025] The atmosphere preparation includes evacuating the furnace and backfilling the furnace with gas;

[0026] Backfill gas includes nitrogen;

[0027] The nitrogen partial pressure is greater than 10 kPa and continues until before step d.

[0028] Furthermore, step c is accompanied by a furnace temperature of 1600-1900°C.

[0029] Furthermore, the support layer has a thickness of 100-1000 μm.

[0030] A method for preparing a low-resistance composite substrate comprises: preparing a support layer and a donor layer, performing ion implantation on a surface of the donor layer, forming a weakened layer at a certain depth of the surface, wherein the weakened layer divides the donor layer into a film layer and a layer to be recycled;

[0031] The step also includes transferring the film layer to a support layer to form the film layer on the support layer;

[0032] The support layer is the support layer mentioned above.

[0033] Furthermore, the step of forming a film layer on the support layer includes: bonding the film layer surface of the donor layer to the support layer to form a bonded body;

[0034] Stress is applied to the bonding body to crack the weakened layer, thereby forming a film layer on the support layer.

[0035] Furthermore, the method further includes the step of performing surface treatment on the layer to be recycled so that the layer to be recycled forms a new donor layer.

[0036] Beneficial effects of the present invention:

[0037] The low-resistance composite substrate structure and manufacturing method provided by the present application, the supporting substrate is 3C-type SiC single crystal, manufactured by liquid phase method, and the resistivity is less than 1mΩ·cm, which meets the low resistivity requirements of the industry. The composite substrate of the present invention has a very low resistivity of the supporting substrate, and the back thinning amount is greatly reduced, and even the back thinning step is not required, which greatly reduces the manufacturing cycle and cost of power devices, and can also avoid damage to the device due to thinning, thereby improving the device yield. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 It is a schematic diagram of the structure of the composite substrate of the present invention;

[0039] Figure 2 It is a schematic diagram of the preparation process of the composite substrate of the present invention;

[0040] Figure 3 It is a schematic diagram of the structure of the preparation device of the present invention;

[0041] In the figure: 1, donor layer; 2, support layer; 3, membrane layer; 4, weakened layer; 1', layer to be recovered; 11, seed crystal rod; 12, seed crystal holder; 13, seed crystal; 14, crystal; 15, alloy solution; 16, graphite crucible; 17, crucible axis. DETAILED DESCRIPTION

[0042] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention, rather than to limit the present invention.

[0043] Example 1

[0044] See also Figure 1-3 , this embodiment provides a method for preparing a low-resistance composite substrate, including preparing a donor layer 1 and a support layer 2, wherein the material of the donor layer 1 is single-crystalline silicon carbide of 4H crystal form, and the material of the support layer 2 is single-crystalline silicon carbide of 3C crystal form. Ions are implanted inward from one surface of the donor layer 1 to form a weakened layer 4 in the donor layer 1, and the weakened layer 4 divides the donor layer 1 into a film layer 3 and a layer 1' to be recycled. The film layer 3 side of the donor layer 1 is bonded to the support layer 2 to form a bonded body. The bonded body is heat-treated to cause the donor layer 1 to crack along the weakened layer 4, so that the film layer 3 is transferred to the support layer 2, forming a composite substrate formed by the support layer 2 and the film layer 3. The layer 1' to be recycled is recycled as a new donor layer 1 after surface treatment until it is exhausted.

[0045] The support layer 2 is obtained by cutting, thinning, grinding and polishing the crystal grown by the liquid phase method. The process of growing crystal by the liquid phase method includes: providing a crystal preparation device, including a furnace body, a graphite crucible 17 for holding raw materials is arranged in the furnace body, a seed crystal rod 11 is arranged above the graphite crucible 17, a seed crystal holder 12 is arranged at one end of the seed crystal rod 11, and a silicon carbide seed crystal 13 is arranged on the seed crystal holder 12, and also includes a heating device for providing the required temperature for preparation, and an atmosphere device for providing the required atmosphere environment for preparation, such as evacuating the furnace and introducing high-pressure gas into the furnace.

[0046] Relying on the above-mentioned crystal preparation device, the crystal is prepared through the following preparation steps:

[0047] a. Loading: Mix the raw materials evenly and put them in a graphite crucible. The raw materials include 50% Si, 40% Cr, and 10% of the rest by mass, and the rest includes Al, Ti, Sc, Ni, Co, Mn, Mg, Ge, As, Dy, Y, Nb, Nd, and Fe.

[0048] a'Preparation of atmosphere environment: After evacuating the furnace, backfill with gas, including Ar and nitrogen, until the pressure in the furnace reaches 50 kPa, of which the nitrogen partial pressure is 10 kPa.

[0049] b. Chemical material: heating the raw materials to melt them and form alloy solution;

[0050] c Growth: Rise and rotate the seed crystal rod to pull the crystal to obtain the crystal. During the growth process, the temperature in the furnace is maintained at around 1800℃ and must not be higher than 1900℃.

[0051] d. Preparation of support layer: The crystal is cut, thinned, ground and polished to obtain support layer 2.

[0052] The thickness of the support layer 2 is 350 μm. After measurement, the crystal form of the support layer 2 is 3C type, the maximum in-plane resistivity is 0.9 mΩ·cm, and the nitrogen doping concentration is 1.5E20atom / cm 3 The roughness of the bonding surface of the polished support layer 2 is less than 0.2 nm, and it can be well bonded with the film layer 3 to obtain a composite substrate of good quality.

[0053] During the preparation of crystals, maintaining a high nitrogen partial pressure in the furnace will affect the solubility of nitrogen in the cosolvent, thereby affecting the wettability between the cosolvent and the seed crystal, thereby affecting the crystal form of the growing crystal. If the nitrogen partial pressure is lower than 10kPa, the wetting angle between the cosolvent and 3C crystal SiC is larger than the wetting angle of other crystal SiC, and the growing crystal is more inclined to other crystal forms other than 3C, so that the growing crystal contains or is entirely crystalline SiC other than 3C, and the resistivity of at least part or all of the supporting layer after processing is greater than 10mΩ·cm; when the nitrogen partial pressure is greater than 10kPa, the wetting angle between the cosolvent and 3C crystal SiC is smaller than the wetting angle of other crystal SiC, and the growing crystal is more inclined to 3C crystal form, and SiC that is entirely 3C crystal form can be obtained. After processing, the resistivity of the substrate in all areas is less than 1mΩ·cm. The nitrogen partial pressure is also not easy to be too high, which will lead to an increase in the defect density in the crystal.

[0054] The growth temperature is controlled to be no more than 1900° C. If the temperature is too high, the crystal type of the grown crystal will tend to 4H or 6H, so that the grown crystal contains or is entirely crystalline SiC other than 3C, and the resistivity of at least a part or all of the supported layer after processing is greater than 10 mΩ·cm.

[0055] Example 2

[0056] The difference from Example 1 is that in step a', the furnace is evacuated and then backfilled with gas, the gas comprising Ar and nitrogen, until the pressure in the furnace reaches 100 kPa, wherein the nitrogen partial pressure is 20 kPa.

[0057] The thickness of the prepared support layer 2 is 350 μm. After measurement, the support layer 2 has a 3C crystal form, a maximum in-plane resistivity of 0.7 mΩ·cm, and a nitrogen doping concentration of 1.8E20atom / cm 3 .

[0058] Example 3

[0059] The difference from Example 1 is that in step a', the furnace is evacuated and then backfilled with gas, the gas comprising Ar and nitrogen, until the pressure in the furnace reaches 200 kPa, wherein the nitrogen partial pressure is 70 kPa.

[0060] The thickness of the prepared support layer 2 is 350 μm. After measurement, the support layer 2 has a 3C crystal form, a maximum in-plane resistivity of 0.5 mΩ·cm, and a nitrogen doping concentration of 2.1E20 atom / cm 3 .

[0061] Example 4

[0062] The difference from Example 1 is that in step a', the furnace is evacuated and then backfilled with gas, which is nitrogen, until the pressure in the furnace reaches 100 kPa.

[0063] The thickness of the prepared support layer 2 is 350 μm. After measurement, the support layer 2 has a 3C crystal form, a maximum in-plane resistivity of 0.2 mΩ·cm, and a nitrogen doping concentration of 2.5E20atom / cm 3 .

[0064] Comparative Example 1

[0065] The difference from Example 1 is that in step a', the furnace is evacuated and then backfilled with gas, the gas comprising Ar and nitrogen, until the pressure in the furnace reaches 50 kPa, wherein the nitrogen partial pressure is 5 kPa.

[0066] The thickness of the prepared support layer 2 is 350 μm. After measurement, the crystal form of the support layer 2 is 4H crystal form, and the maximum in-plane resistivity is 10 mΩ·cm. Due to the high resistivity of the support layer, the vertical on-resistance of the device prepared by the composite substrate is large.

[0067] Comparative Example 2

[0068] The difference from Example 1 is that the support layer of the composite substrate is polycrystalline silicon carbide with a resistivity of 2 mΩ·cm.

[0069] Due to the high resistivity of the support layer, the vertical on-resistance of the device prepared by the composite substrate is large. The support layer is polycrystalline silicon carbide, and the roughness of the bonding interface after treatment is still higher than 1nm, resulting in poor bonding effect between the support layer and the film layer and poor quality of the composite substrate.

[0070] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, various obvious changes, readjustments and substitutions can be made without departing from the protection scope of the present invention. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A low-resistance composite substrate structure, characterized in that: It includes a support layer and a film layer formed on the support layer; The film layer is single crystal silicon carbide, and the crystal form is 4H type; The support layer is single crystal silicon carbide, and the crystal form is 3C type; The resistivity of the support layer is less than 1 mΩ·cm.

2. The composite substrate structure according to claim 1, characterized in that: The nitrogen doping concentration of the support layer is 1.5-2.5E20atom / cm 3 .

3. The composite substrate structure according to claim 1, characterized in that: The support layer is prepared by a liquid phase method, and the preparation relies on a preparation device, which includes a furnace body; A graphite crucible for containing raw materials is provided in the furnace body; A seed crystal rod is provided above the graphite crucible; A seed crystal holder is arranged at one end of the seed crystal rod, and a silicon carbide seed crystal is arranged on the seed crystal holder; A heating device, used to provide the temperature required for preparation; The atmosphere device is used to provide the atmosphere environment required for preparation.

4. The composite substrate structure according to claim 3, characterized in that: The preparation method of the support layer comprises: a. Loading: Mix the raw materials evenly and put them in a graphite crucible; b. Chemical material: heating the raw materials to melt them and form alloy solution; c. Growth: ascending and rotating the seed crystal rod to pull and grow the crystal to obtain the crystal; d. Prepare the support layer: cut, thin, grind and polish the crystal to obtain the support layer.

5. The composite substrate structure according to claim 4, characterized in that: After step a, it also includes atmosphere preparation; The atmosphere preparation includes evacuating the furnace and backfilling the furnace with gas; Backfill gases include nitrogen; The nitrogen partial pressure is greater than 10 kPa and continues until before step d.

6. The composite substrate structure according to claim 4, characterized in that: The furnace temperature during step c is 1600-1900°C.

7. The composite substrate structure according to claim 4, characterized in that: The support layer has a thickness of 100-1000 μm.

8. A method for preparing a low-resistance composite substrate, characterized in that: Prepare a support layer and a donor layer, perform ion implantation on a surface of the donor layer, and form a weakened layer at a certain depth of the surface, wherein the weakened layer divides the donor layer into a film layer and a layer to be recycled; The step also includes transferring the film layer to a support layer to form the film layer on the support layer; The support layer is the support layer described in any one of claims 1-7.

9. The preparation method according to claim 8, characterized in that: The step of forming a film layer on the support layer includes: bonding the film layer surface of the donor layer to the support layer to form a bonded body; Stress is applied to the bonding body to crack the weakened layer, thereby forming a film layer on the support layer.

10. The preparation method according to claim 9, characterized in that: The method also includes a step of performing surface treatment on the layer to be recycled so that the layer to be recycled forms a new donor layer.