BN fiber-based composite material and preparation method thereof

By preparing BN fiber-based composite materials with mesoporous and microporous, the problem of targeted monitoring of antibiotics by existing adsorbents and low adsorption capacity is solved, efficient adsorption and rapid desorption of pollutants are achieved, and resource waste is reduced and environmental pollution.

CN118895580APending Publication Date: 2024-11-05XIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410985920.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing adsorbents cannot be targeted monitoring of antibiotics, have low adsorption capacity and cannot be quickly desorbed, resulting in waste of resources and environmental pollution.

Method used

By preparing BN fiber-based composite materials with internal mesoporous and surface micropores, the specific surface area and adsorption capacity of boron nitride fibers are improved by using pore-forming agents, surface plasma etching and irradiation grafting techniques, and the specific surface area and adsorption capacity of boron nitride fibers are improved, and color development single The body realizes targeted monitoring of pollutants and rapid absorption/desorption of pollutants.

Benefits of technology

Efficient targeted monitoring and rapid adsorption/desorption of antibiotics are achieved, the adsorption volume is increased, resource waste is reduced, and the performance of materials is maintained well when reused.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895580A_ABST
    Figure CN118895580A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a BN (boron nitride) fiber-based composite material, which comprises the following steps: adding a pore-forming agent into a precursor solution, performing surface plasma etching to obtain boron nitride fibers with internal mesopores and surface micropores, grafting a polymer on the surfaces of the boron nitride fibers through irradiation grafting, and introducing a color developing monomer, thereby obtaining the BN fiber-based composite material. The BN fiber-based composite material is successfully prepared; according to the BN fiber-based composite material prepared by the preparation method disclosed by the invention, the adsorption capacity of the BN fiber-based composite material on pollutants is greatly improved by virtue of a multi-scale pore structure, and the BN fiber-based composite material is not easy to block in a pollutant adsorption / desorption process and is convenient to reuse; the polymer chain shrinks and stretches by releasing particles with different electrical properties, so that rapid adsorption / desorption of pollutants is realized; the color developing monomer monitors the concentration of TC in the sewage in a targeted manner through a fluorescence reaction, so that the BN fiber-based composite material can be properly used, and resources are saved; the BN fiber-based composite material has wide application prospects in the fields of sewage treatment, agricultural irrigation, food analysis and monitoring and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adsorption materials, and in particular to a BN fiber-based composite material and a preparation method thereof. Background Art

[0002] In the development of global agriculture, the use of wastewater for agricultural irrigation is a beneficial practice that is in line with the goals of sustainable development. However, new pollutants such as antibiotics in wastewater will spread into the soil, affect soil microorganisms, and be absorbed and accumulated by crops, ultimately posing a serious threat to public food safety. Therefore, the development of adsorbent materials that have targeted monitoring functions for antibiotics in sewage, can quickly adsorb them in large quantities, and can quickly remove them after adsorption is crucial for agricultural development and food safety. At present, the widely used adsorbent materials are mainly concentrated in: carbon material adsorbent materials, polymer adsorbent materials and mineral adsorbent materials. Researchers mainly design their structures or add functional particles to enable them to have the functions of targeted monitoring and large-scale adsorption of pollutants.

[0003] For example, the Chinese patent "High-efficiency targeted adsorbent for treating perchlorate wastewater and its preparation method and application" (application number: 202311720740.8, application publication number: CN 117920168A, publication date: 2024.04.26) discloses a high-efficiency targeted adsorbent with a surface of a porous crustacean biomass matrix and a modified material loaded in the pore structure. By modifying the adsorbent material, the surface properties of the surface and the internal voids are optimized, so that the adsorbent material is positively charged as a whole, and becomes a carrier for adsorbing perchlorate in the water body, so that the material is suitable for a wide range of wastewater pH, and the adsorption capacity and adsorption selectivity for perchlorate are improved. However, the pore surface of the adsorbent matrix surface is easily covered after multiple adsorptions, making the activation system loaded inside unable to function, thereby losing the function of targeted adsorption.

[0004] The Chinese patent "A targeted adsorption catalyst, its preparation method and application" (application number: 202311257927.9, application publication number: CN 117299205 A, publication date: 2023.12.29) discloses an adsorption catalyst in which a molecular imprinting polymer is loaded on activated carbon loaded with manganese oxide, wherein the molecular imprinting polymer achieves targeted recognition of the target molecule by constructing a selective recognition site of the target molecule (SPY); the manganese oxide catalytic active site can catalyze the active oxidant, thereby generating free radicals with strong oxidizing effect to degrade the target pollutant. However, the adsorbent cannot determine whether the sewage contains the target molecule, and cannot accurately quantify the amount of catalyst to be added, which is easy to cause resource waste and environmental pollution.

[0005] The Chinese patent "A preparation method of a boron nitride adsorbent material, the prepared adsorbent material and its application" (application number: 202210176032.1, application announcement number: CN 114669266A, announcement date: 2022.06.28) discloses a preparation method of a boron nitride adsorbent material, which has a large specific surface area and a large number of functional groups on the surface. The boron nitride adsorbent material can achieve efficient adsorption of heavy metal ions. However, the structure of the boron nitride material is relatively simple, and the space inside the fiber cannot be effectively utilized, making its adsorption capacity for pollutants unsatisfactory.

[0006] Song et al. (Qianqian Song, Jianli Liang, Yi Fang, et al. Nickel (II) modified porous boron nitride: An effective adsorbent for tetracycline removal from aqueous solution. Chemical Engineering Journal, 2020, 394, 124985) loaded Ni (II) as a modifier on the porous BN surface, and the Ni (II) modified multi-BN had a removal rate of TC of up to 99.769%, far exceeding the original porous BN (70.853%) and most other reported adsorption materials. However, the specific surface area of ​​the adsorbent is not high, which makes its adsorption capacity poor, and the adsorbent removes pollutants by high-temperature calcination, making the desorption process cumbersome. Summary of the invention

[0007] The object of the present invention is to provide a BN fiber-based composite material and a preparation method thereof, so as to solve the technical problems that the existing adsorbents cannot perform targeted monitoring on antibiotics, have low adsorption capacity, and cannot rapidly desorb.

[0008] In order to achieve the above object, the technical solution adopted by the present invention is:

[0009] A method for preparing a BN fiber-based composite material is specifically implemented by the following steps:

[0010] Step 1, preparation of mesoporous boron nitride fibers:

[0011] Firstly, a boron source, a nitrogen source and a pore-forming agent are added to a solvent in proportion, and a boron nitride precursor is obtained by pyrolysis of the precursor, extraction and freeze drying, and then the boron nitride precursor is calcined at a high temperature to obtain a boron nitride fiber with a large number of mesopores inside.

[0012] Step 2, preparation of microporous boron nitride fibers:

[0013] The boron nitride fiber obtained in step 1 is subjected to surface plasma etching to obtain a boron nitride fiber having a large number of microporous structures on the surface;

[0014] Step 3, surface modification:

[0015] The boron nitride fiber obtained in step 2 and the charged coupling agent are subjected to electrophoretic deposition to obtain a modified boron nitride fiber having a large number of free radicals on the surface and the modified boron nitride fiber is stored in a refrigerator;

[0016] Step 4, irradiation grafting:

[0017] The modified boron nitride fiber, polymer monomer, color-developing monomer and initiator obtained in step 3 are added into deionized water, and the boron nitride fiber grafted with two polymers is obtained under the irradiation of ultraviolet light.

[0018] Furthermore, in step 1, the boron source is one of boric acid, boric acid amine, and sodium borohydride, the nitrogen source is one of melamine, ammonia, and urea, the pore-forming agent is one of brominated alkylamine, quaternary ammonium salt, nitrobenzene sulfonate, sulfate ester salt, polyethylene glycol, and octylphenol polyoxyethylene ether, the solvent is one of deionized water, ethanol, acetone, dimethylformamide, and tert-butanol, and the molar ratio of the boron source, the nitrogen source, and the pore-forming agent is 15-20:1-3:0.5-2;

[0019] In the precursor pyrolysis method, the temperature of the reaction liquid water area is 80-90°C, the insulation time is 30-60min, the stirring speed is 200-300r, and the boron nitride precursor is filtered and freeze-dried for 12-24h;

[0020] The specific method of high-temperature calcination is as follows: the boron nitride precursor is calcined in a tubular furnace filled with inert gas, the calcination temperature is 1300-1500°C, the inert gas is one of nitrogen and argon, and the insulation time is 2-5 hours.

[0021] Furthermore, in step 2, the voltage and power of the surface plasma etching of the boron nitride fiber are 15-20 kV and 5-10 W respectively, and the etching time is 20-40 min.

[0022] Furthermore, the specific method of step 3 is: first, dissolve the charged coupling agent in isopropanol to form a charged coupling agent solution, then immerse the boron nitride fiber in the charged coupling agent solution, and deposit it at a voltage of 5 to 10 kV for 30 to 50 minutes, and finally filter the boron nitride fiber, wash it with ethanol and deionized water, and dry it to obtain modified boron nitride fiber, which is refrigerated at 0 to 10°C.

[0023] Furthermore, in step 3, the charged coupling agent is one of an amino coupling agent, an amine coupling agent, a carboxyl coupling agent, and a sulfonic acid coupling agent.

[0024] Furthermore, the specific method of step 4 is: first, the modified boron nitride fiber, polymer monomer, and initiator are added to deionized water, irradiated and grafted for 20 to 40 minutes, then the product is centrifuged, washed with ethanol and deionized water to obtain the boron nitride fiber grafted with the polymer, and finally the boron nitride fiber grafted with the polymer, the color-developing monomer, the initiator, and the oxidized hydrochloric acid are added to 100 to 200 mL of dimethyl sulfoxide and reacted in an ice bath to obtain the boron nitride fiber grafted with the two polymers through the reaction.

[0025] Furthermore, in step 4, the polymer monomer is one of methacrylate, dimethylaminoethylamine, acrylic acid, and methyl methacrylate, the color-developing monomer is benzaldehyde and methylenetriphenylphosphine, and the initiator is AIBN.

[0026] The BN fiber-based composite material is prepared according to the above-mentioned method for preparing a BN fiber-based composite material.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] A BN fiber-based composite material capable of targeted monitoring and rapid adsorption / desorption of pollutants. Boron nitride fibers with internal mesopores, surface micropores and grafted polymers and color-developing monomers are obtained by adding pore-forming agents, surface plasma etching, irradiation grafting, etc. The internal mesopores greatly increase the specific surface area of ​​the boron nitride fiber, thereby greatly increasing the adsorption capacity of the fiber for pollutants, and the fiber is not easily blocked during the process of adsorption / desorption of pollutants, thus facilitating reuse; the surface micropores enable the polymer and the color-developing monomer to be evenly and firmly embedded in the surface of the boron nitride, and the polymer chain achieves rapid adsorption / desorption of pollutants by releasing particles of different electrical properties and structural contraction and expansion; the color-developing monomer targets and monitors the concentration of TC in sewage through fluorescence reaction, so that the BN fiber-based composite material can be used appropriately and resources can be saved; the BN fiber-based composite material has broad application prospects in the fields of sewage treatment, agricultural irrigation, and food analysis and monitoring. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic diagram of the morphology of a single fiber of the BN fiber-based composite material prepared by the present invention.

[0030] In the attached figure, 1-internal mesopores, 2-surface micropores, 3-grafted polymer, 4-chromogenic monomer. DETAILED DESCRIPTION

[0031] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0032] A method for preparing a BN fiber-based composite material capable of targeted monitoring and rapid adsorption / desorption of pollutants is specifically implemented in the following steps.

[0033] Step 1, preparation of mesoporous boron nitride fibers:

[0034] A boron source, a nitrogen source and a pore-forming agent are added to a solvent in proportion, and a boron nitride precursor is obtained by filtration and freeze-drying through a precursor pyrolysis method, wherein the boron source is one of boric acid, boric acid amine and sodium borohydride, the nitrogen source is one of melamine, ammonia water and urea, and the pore-forming agent is a brominated alkylamine, a quaternary ammonium salt, nitrobenzene sulfonate, a sulfate ester salt, polyethylene glycol, octylphenol polyoxyethylene ether, etc.; the molar ratio of the boron source, the nitrogen source and the pore-forming agent is 15-20:1-3:0.5-2, the amount of the solvent is 200-500 mL, and the solvent used is one of deionized water, ethanol, acetone, dimethylformamide and tert-butanol; in the precursor pyrolysis method, the reaction liquid water temperature is 80-90°C, the insulation time is 30-60min, the stirring speed is 200-300r, and the boron nitride precursor is filtered and freeze-dried for 12-24h. Subsequently, the boron nitride precursor is calcined at high temperature to obtain boron nitride fibers with a large number of mesopores inside. The high-temperature calcination of the boron nitride precursor is carried out in a tubular furnace filled with inert gas. The calcination temperature is 1300-1500°C. The inert gas is one of nitrogen and argon. The insulation time is 2-5 hours.

[0035] Step 2, preparation of microporous boron nitride fibers:

[0036] The boron nitride fiber obtained in step 1 is subjected to surface plasma etching under the conditions of voltage and power of 15-20 kV and 5-10 W respectively and etching time of 20-40 min to obtain a boron nitride fiber with a large number of microporous structures on the surface.

[0037] Step 3, surface modification:

[0038] 1-2g of a charged coupling agent is dissolved in 50mL of isopropanol to form a charged coupling agent solution, wherein the charged coupling agent is one of an amino coupling agent, an amine coupling agent, a carboxyl coupling agent, and a sulfonic acid coupling agent. Subsequently, 2-3g of the boron nitride fiber obtained in step 2 is soaked in the charged coupling agent solution, and electrophoretically deposited at a voltage of 5-10kV for 30-50min. Finally, the boron nitride fiber is filtered, washed with ethanol and deionized water, and vacuum dried to obtain a modified boron nitride fiber, which is refrigerated at 0-10°C to obtain a boron nitride fiber with a large number of free radicals on the surface.

[0039] Step 4, irradiation grafting:

[0040] First, the modified boron nitride fiber, polymer monomer and initiator obtained in step 3 are added to deionized water, and the grafting is irradiated under ultraviolet light for 20 to 40 minutes. The product is then centrifuged and washed with ethanol and deionized water to obtain the boron nitride fiber grafted with the polymer; finally, the boron nitride fiber grafted with the polymer, 0.1 to 0.3 g of color-developing monomer, 0.1 g of initiator and hydrochloric acid are added to 100 to 200 mL of dimethyl sulfoxide and reacted in an ice bath to obtain the boron nitride fiber grafted with two polymers, wherein the polymer monomers are methacrylate and dimethylaminoethylamine, acrylic acid and methyl methacrylate, the color-developing monomers are benzaldehyde and methylenetriphenylphosphine, and the initiator is AIBN.

[0041] The present invention successfully prepares a boron nitride fiber with a large number of internal mesopores and surface micropores by adding a pore-forming agent to a boron nitride precursor solution, high-temperature calcination, surface plasma etching treatment, and the like. By controlling the amount of pore-forming agent added, the size and content of the mesopores can be adjusted, which is beneficial to increasing the specific surface area of ​​the boron nitride fiber and improving the adsorption capacity of boron nitride to pollutants; secondly, by controlling the voltage and etching time of surface plasma etching, micropores suitable for grafting polymers and color-developing monomers can be introduced on the surface of the boron nitride fiber; finally, the polymer and the color-developing monomer are uniformly and firmly grafted in the micropores on the surface of the boron nitride fiber through irradiation grafting, and the polymer releases particles of different electrical properties through protonation and deprotonation reactions, and the structure shrinks and stretches, so that TC in the sewage is attracted / repelled to the vicinity / periphery of the boron nitride fiber, and the rapid adsorption and desorption of TC by boron nitride is realized, and the grafted color-developing monomer can realize targeted monitoring of pollutants in sewage through fluorescence reaction.

[0042] Figure 1 Schematic diagram of the cross-sectional morphology of a single BN fiber-based composite material prepared by the present invention. Figure 1 It can be seen that the boron nitride fiber has a large number of internal mesopores 1 with different orientations that penetrate the fiber, and the surface micropores 2 are uniformly inlaid with grafted polymers 3 and color-developing monomers 4.

[0043] Example 1

[0044] First, 15M boric acid, 1M melamine, and 0.5M bromoalkylamine were added to 200mL deionized water to form a reaction solution. The reaction solution was kept warm in an 80°C water environment for 30min with a stirring speed of 200r. The white flocculent product was then filtered and freeze-dried for 12h. Finally, it was kept warm at 1300°C for 2h in a tubular furnace filled with nitrogen atmosphere to obtain mesoporous boron nitride fibers.

[0045] The obtained mesoporous boron nitride fiber was placed in a plasma etching device and etched for 20 minutes under the conditions of an etching voltage of 15 kV and a power of 5 W to obtain a surface microporous boron nitride fiber.

[0046] 1 g of amino coupling agent was dissolved in 50 mL of isopropanol to form a charged coupling agent solution, 2 g of boron nitride fiber was soaked in the charged coupling agent solution, and electrophoretic deposition was performed at a voltage of 5 kV for 30 minutes. After the deposition, the boron nitride fiber was filtered, washed with ethanol and deionized water, and vacuum dried to obtain modified boron nitride fiber, which was refrigerated at 2°C to obtain boron nitride fiber with a large number of free radicals on the surface.

[0047] 2g of modified boron nitride fiber, 1g of methyl methacrylate, and 0.1g of AIBN were added to 200mL of deionized water, and the grafting was carried out by ultraviolet irradiation for 20 minutes. The product was then centrifuged and washed with ethanol and deionized water to obtain boron nitride fiber grafted with polymer; finally, the obtained boron nitride fiber grafted with polymer and 0.1g of benzaldehyde, 0.1g of methylenetriphenylphosphine, 0.1g of AIBN, and 20mL of hydrochloric acid were added to 100mL of dimethyl sulfoxide and allowed to react in an ice bath to obtain boron nitride fiber grafted with two polymers.

[0048] Example 2

[0049] First, 17M boric acid amine, 1.5M urea, and 1M sodium nitrobenzene sulfonate were added to 300mL ethanol to form a reaction solution. The reaction solution was kept warm in an aquatic environment at 85°C for 40min with a stirring speed of 250r. The white flocculent product was then filtered and freeze-dried for 15h. Finally, it was kept warm at 1300°C for 3h in a tubular furnace filled with nitrogen atmosphere to obtain mesoporous boron nitride fibers.

[0050] The obtained mesoporous boron nitride fiber was placed in a plasma etching device and etched for 30 minutes under the conditions of an etching voltage of 17 kV and a power of 7 W to obtain a surface microporous boron nitride fiber.

[0051] 1g of amine coupling agent was dissolved in 50mL of isopropanol to form a charged coupling agent solution, 2g of boron nitride fiber was soaked in the charged coupling agent solution, and electrophoretic deposition was performed at a voltage of 7kV for 40min. After the deposition, the boron nitride fiber was filtered, washed with ethanol and deionized water, and vacuum dried to obtain modified boron nitride fiber, which was refrigerated at 6°C to obtain boron nitride fiber with a large number of free radicals on the surface.

[0052] 2g of modified boron nitride fiber, 1g of dimethylaminoethylamine, and 0.1g of AIBN were added to 200mL of deionized water, and the grafting was carried out under ultraviolet irradiation for 30 minutes. The product was then centrifuged and washed with ethanol and deionized water to obtain boron nitride fiber grafted with polymer; finally, the obtained boron nitride fiber grafted with polymer and 0.2g of benzaldehyde, 0.2g of methylenetriphenylphosphine, 0.1g of AIBN, and 20mL of hydrochloric acid were added to 150mL of dimethyl sulfoxide and allowed to react in an ice bath to obtain boron nitride fiber grafted with two polymers.

[0053] Example 3

[0054] First, 18M sodium borohydride, 2M ammonia water, and 1.5M quaternary ammonium salt were added to 400mL acetone to form a reaction solution. The reaction solution was kept warm in an 87°C water environment for 50min with a stirring speed of 270r. The white flocculent product was then filtered and freeze-dried for 20h. Finally, it was kept warm at 1400°C for 4h in a tubular furnace filled with nitrogen atmosphere to obtain mesoporous boron nitride fibers.

[0055] The obtained mesoporous boron nitride fiber was placed in a plasma etching device and etched for 35 minutes under the conditions of an etching voltage of 19 kV and a power of 8 W to obtain a surface microporous boron nitride fiber.

[0056] 1 g of carboxyl coupling agent was dissolved in 50 mL of isopropanol to form a charged coupling agent solution, 2 g of boron nitride fiber was immersed in the charged coupling agent solution, and electrophoretic deposition was performed at a voltage of 8 kV for 45 minutes. After the deposition, the boron nitride fiber was filtered, washed with ethanol and deionized water, and vacuum dried to obtain modified boron nitride fiber, which was refrigerated at 0°C to obtain boron nitride fiber with a large number of free radicals on the surface.

[0057] 2g of modified boron nitride fiber, 1g of acrylic acid, and 0.1g of AIBN were added to 200mL of deionized water, and the grafting was carried out by ultraviolet irradiation for 35min. The product was then centrifuged and washed with ethanol and deionized water to obtain boron nitride fiber grafted with polymer; finally, the obtained boron nitride fiber grafted with polymer and 0.3g of benzaldehyde, 0.3g of methylenetriphenylphosphine, 0.1g of AIBN, and 20mL of hydrochloric acid were added to 180mL of dimethyl sulfoxide, and allowed to react in an ice bath to obtain boron nitride fiber grafted with two polymers.

[0058] Example 4

[0059] First, 20M boric acid, 3M melamine, and 2M sulfate were added to 500mL dimethylformamide to form a reaction solution. The reaction solution was kept warm in a 90°C water environment for 60min with a stirring speed of 300r. The white flocculent product was then filtered and freeze-dried for 24h. Finally, it was kept warm at 1500°C for 5h in a tubular furnace filled with argon atmosphere to obtain mesoporous boron nitride fibers.

[0060] The obtained mesoporous boron nitride fiber was placed in a plasma etching device and etched for 40 minutes under the conditions of an etching voltage of 20 kV and a power of 10 W to obtain a surface microporous boron nitride fiber.

[0061] 2g of sulfonic acid coupling agent is dissolved in 50mL of isopropanol to form a charged coupling agent solution, 3g of boron nitride fiber is soaked in the charged coupling agent solution, and electrophoretic deposition is performed at a voltage of 10kV for 50min. After the deposition, the boron nitride fiber is filtered, washed with ethanol and deionized water, and vacuum dried to obtain modified boron nitride fiber, which is refrigerated at 10°C to obtain boron nitride fiber with a large number of free radicals on the surface.

[0062] 2g of modified boron nitride fiber, 1g of methyl methacrylate, and 0.1g of AIBN were added to 200mL of deionized water, and the grafting was carried out by ultraviolet irradiation for 40 minutes. The product was then centrifuged and washed with ethanol and deionized water to obtain boron nitride fiber grafted with polymer; then the obtained boron nitride fiber grafted with polymer and 0.3g of benzaldehyde, 0.3g of methylenetriphenylphosphine, 0.1g of AIBN, and 20mL of hydrochloric acid were added to 200mL of dimethyl sulfoxide, and allowed to react in an ice bath to obtain boron nitride fiber grafted with two polymers.

[0063] After 100 mL of a mixed solution containing 50 mg / L tetracycline and 50 mg / L sulfapyridine was added with 10 mg of the BN fiber-based composite material prepared in Examples 1 to 4 for adsorption for 4 hours, the average removal rates of tetracycline and sulfapyridine reached 97.52% and 10.37%, respectively, indicating that the BN fiber-based composite material prepared by the present invention has a very high adsorption effect on tetracycline, but a very low adsorption effect on sulfapyridine, that is, the adsorbent has a targeted adsorption function for tetracycline. Compared with other targeted adsorbents (Chinese patent "A targeted adsorption catalyst, its preparation method and application" (application number: 202311257927.9, application publication number: CN 117299205 A, publication date: 2023.12.29), the BN fiber-based composite adsorbent prepared by the present invention has a stronger targeted adsorption ability for pollutants and a larger adsorption capacity.

[0064] To 100mL solution containing 100mg / L tetracycline, 10mg of the BN fiber-based composite material prepared in Examples 1 to 4 and 10mL of HCl were added respectively. After 4 hours of adsorption, the average adsorption rate of tetracycline reached 90%; as a control group, 10mg of the BN fiber-based composite material prepared in Examples 1 to 4 was added to 100mL solution containing 100mg / L tetracycline respectively. After 4 hours of adsorption, the average adsorption rate of tetracycline reached 60%. It can be seen that when HCl is added to the mixed solution, the pH-responsive polymer in the BN fiber-based composite material can be protonated, positive ions are released, and the side chains shrink, so that more fiber surfaces are exposed to tetracycline in the solution, and the tetracycline is firmly adsorbed in the microporous structure inside the fiber.

[0065] After the adsorption, the BN fiber-based composite materials were washed and dried, and added to 1.25 mol / L NaOH solution, ultrasonically dispersed, and allowed to stand for 5 min. The adsorbent was then washed and dried and recovered. 5 mg of the recovered BN fiber-based composite materials were added to 50 mL of a solution containing 100 mg / L tetracycline, and 5 mL of HCl was added. After four hours of adsorption, the average adsorption rate of tetracycline reached 89%. As a control group, 5 mg of the recovered adsorbent was added to a 50 mL solution containing 100 mg / L tetracycline. After four hours of adsorption, the average adsorption rate of tetracycline reached 58%. It can be seen that in an alkaline environment, the adsorbed pollutants can be removed in large quantities through pH response, and the adsorption performance of the BN fiber-based composite materials is almost unaffected after recovery.

[0066] The above-mentioned embodiments only express the specific implementation of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims.

Claims

1. A method for preparing a BN fiber-based composite material, characterized in that: Follow the steps below to implement it: Step 1, preparation of mesoporous boron nitride fibers: Firstly, a boron source, a nitrogen source and a pore-forming agent are added to a solvent in proportion, and a boron nitride precursor is obtained by pyrolysis of the precursor, extraction and freeze drying, and then the boron nitride precursor is calcined at a high temperature to obtain a boron nitride fiber with a large number of mesopores inside. Step 2, preparing microporous boron nitride fibers: The boron nitride fiber obtained in step 1 is subjected to surface plasma etching to obtain a boron nitride fiber having a large number of microporous structures on the surface; Step 3, surface modification: The boron nitride fiber obtained in step 2 and the charged coupling agent are subjected to electrophoretic deposition to obtain a modified boron nitride fiber having a large number of free radicals on the surface and the modified boron nitride fiber is stored in a refrigerator; Step 4, irradiation grafting: The modified boron nitride fiber, polymer monomer, color-developing monomer and initiator obtained in step 3 are added into deionized water, and the boron nitride fiber grafted with two polymers is obtained under the irradiation of ultraviolet light.

2. The method for preparing a BN fiber-based composite material according to claim 1, characterized in that: In step 1, the boron source is one of boric acid, boric acid amine, and sodium borohydride, the nitrogen source is one of melamine, ammonia, and urea, the pore-forming agent is one of brominated alkylamine, quaternary ammonium salt, nitrobenzene sulfonate, sulfate ester salt, polyethylene glycol, and octylphenol polyoxyethylene ether, the solvent is one of deionized water, ethanol, acetone, dimethylformamide, and tert-butanol, and the molar ratio of the boron source, the nitrogen source, and the pore-forming agent is 15-20:1-3:0.5-2; In the precursor pyrolysis method, the temperature of the reaction liquid water area is 80-90°C, the insulation time is 30-60min, the stirring speed is 200-300r, and the boron nitride precursor is filtered and freeze-dried for 12-24h; The specific method of high-temperature calcination is as follows: the boron nitride precursor is calcined in a tubular furnace filled with inert gas, the calcination temperature is 1300-1500°C, the inert gas is one of nitrogen and argon, and the insulation time is 2-5 hours.

3. The method for preparing a BN fiber-based composite material according to claim 1, characterized in that: In step 2, the voltage and power of the surface plasma etching of the boron nitride fiber are 15-20 kV and 5-10 W respectively, and the etching time is 20-40 min.

4. The method for preparing a BN fiber-based composite material according to claim 1, characterized in that: The specific method of step 3 is: first, dissolve the charged coupling agent in isopropanol to form a charged coupling agent solution, then immerse the boron nitride fiber in the charged coupling agent solution, and deposit it at a voltage of 5 to 10 kV for 30 to 50 minutes. Finally, filter the boron nitride fiber, wash it with ethanol and deionized water, and dry it to obtain modified boron nitride fiber, which is refrigerated at 0 to 10°C.

5. The method for preparing a BN fiber-based composite material according to claim 4, characterized in that: In step 3, the charged coupling agent is one of an amino coupling agent, an amine coupling agent, a carboxyl coupling agent, and a sulfonic acid coupling agent.

6. The method for preparing a BN fiber-based composite material according to claim 1, characterized in that: The specific method of step 4 is as follows: first, the modified boron nitride fiber, polymer monomer, and initiator are added to deionized water, and irradiated for grafting for 20 to 40 minutes. Then, the product is centrifuged, washed with ethanol and deionized water to obtain the boron nitride fiber grafted with the polymer. Finally, the obtained boron nitride fiber grafted with the polymer, the color-developing monomer, the initiator, and the oxidized hydrochloric acid are added to 100 to 200 mL of dimethyl sulfoxide and reacted in an ice bath to obtain the boron nitride fiber grafted with the two polymers.

7. The method for preparing a BN fiber-based composite material according to claim 6, characterized in that: In step 4, the polymer monomer is one of methacrylate, dimethylaminoethylamine, acrylic acid, and methyl methacrylate, the color-developing monomer is benzaldehyde and methylenetriphenylphosphine, and the initiator is AIBN.

8. A BN fiber-based composite material prepared according to the method for preparing a BN fiber-based composite material according to any one of claims 1 to 7.