High-stripping hydrolysis-resistant waterborne polyurethane synthetic leather

By adding chitosan and isocyanate dispersed components to the aqueous polyurethane synthetic leather, and adding oligomers in combination with active addition, forming a cross-linked structure, the problem of unstable bonding of ultra-fiber synthetic leather for water-based polyurethane foam finishing is solved, and the peeling is significantly improved Strength and service life, achieving environmental protection and energy saving effects.

CN118895673APending Publication Date: 2024-11-05FUJIAN HEXIN SYNTHETIC LEATHER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411180975.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The foam coating of water-based polyurethane foam finishing is relatively high in production of ultra-fiber synthetic leather, resulting in poor bonding, low peel strength and short service life.

Method used

The high peeling and hydrolysis-resistant polyurethane synthetic leather solution is adopted, including the aqueous polyurethane pretreatment base cloth, a modified tackifying intermediate layer and a surface layer. The adhesive structure is formed by adding chitosan and isocyanate dispersed components to the surface layer, and The active addition of oligomers is used to enhance the interface binding force and achieve cross-linking and curing.

Benefits of technology

Significantly improve the peel strength and service life, the peel strength retention rate is greater than 82%, and the dry peel strength is greater than 125N/3cm, achieving green and environmental protection, energy conservation and emission reduction, and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895673A_ABST
    Figure CN118895673A_ABST
Patent Text Reader

Abstract

The invention discloses high-stripping hydrolysis-resistant waterborne polyurethane synthetic leather, and relates to the technical field of polyurethane synthetic materials, and the high-stripping hydrolysis-resistant waterborne polyurethane synthetic leather comprises waterborne polyurethane pretreatment base cloth, a modified tackifying middle layer and a surface layer; the surface layer is obtained by coating release paper with waterborne polyurethane slurry and drying to form a film; the modified tackifying middle layer is formed by coating the surface of the surface layer with an isocyanate dispersed component, carrying out semi-curing treatment, and then laminating, cross-linking and curing with the waterborne polyurethane pre-treated base cloth; wherein the waterborne polyurethane slurry contains chitosan with the mass ratio of 0.5 to 2 percent, and the particle size of the chitosan is 60 to 200nm; the isocyanate dispersion component is prepared from the following components in parts by weight: 40 to 50 parts of diisocyanate, 55 to 70 parts of oligomer polyol, 1 to 3 parts of dihydric alcohol and / or polyol, 0.4 to 1.6 parts of active additive oligomer, 0.01 to 0.5 part of deionized water, 0.1 to 0.2 part of organic silicon surfactant and 0.01 to 0.2 part of intermediate layer catalyst. The adhesive has the effects of remarkably improving the peel strength and prolonging the service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polyurethane synthetic materials, and in particular to a highly peelable and hydrolysis-resistant water-based polyurethane synthetic leather. Background Art

[0002] After decades of development, my country's synthetic leather industry has grown from nothing to a major producer and consumer today. Since early synthetic leather used solvent-based polyurethane, its solvent pollution has gradually attracted attention from all walks of life. Therefore, in recent years, it has become a general trend to gradually use water-based polyurethane to replace solvent-based polyurethane to produce synthetic leather. Although water-based polyurethane synthetic leather is more environmentally friendly than solvent-based polyurethane synthetic leather, its hygienic performance is not as good as natural leather, and its comfort needs to be improved. Therefore, how to increase the water vapor permeability of water-based polyurethane synthetic leather and improve its hygienic performance has become a research direction that has attracted much attention in water-based synthetic leather.

[0003] The Chinese patent application document with publication number CN105239417A discloses a formula and process for producing microfiber synthetic leather by finishing with water-based polyurethane foam. The process is to first produce foam slurry, then directly coat the foam slurry on a microfiber base cloth, and finally perform complex post-finishing steps such as grinding and embossing, and laminating the surface layer with the foamed base using release paper as a carrier to obtain water-based polyurethane microfiber synthetic leather.

[0004] However, in the formula and process of producing microfiber synthetic leather by water-based polyurethane foam finishing, the viscosity of the foam coating is relatively high, and the slurry is not easy to penetrate into the interior of the microfiber base cloth, which will inevitably lead to poor adhesion between the foam coating and the substrate, resulting in a short service life due to low peel strength during application, which needs to be improved. Summary of the invention

[0005] In view of this, the purpose of this application is to provide a highly peelable and hydrolysis-resistant water-based polyurethane synthetic leather to achieve the purpose of significantly improving the peel strength and extending the service life. The specific scheme is as follows:

[0006] A highly peelable and hydrolysis-resistant water-based polyurethane synthetic leather comprises a water-based polyurethane pre-treated base fabric, a modified tackifying intermediate layer and a surface layer; the surface layer is obtained by coating a water-based polyurethane slurry on a release paper and drying to form a film; the modified tackifying intermediate layer is formed by coating an isocyanate dispersed component on the surface of the surface layer, and after semi-curing treatment, it is bonded to the water-based polyurethane pre-treated base fabric and cross-linked and cured; wherein,

[0007] The aqueous polyurethane slurry contains chitosan in a mass ratio of 0.5-2%, and the particle size of the chitosan is 60-200nm; the isocyanate dispersing component includes 40-50 parts by weight of diisocyanate, 55-70 parts by weight of oligomer polyol, 1-3 parts by weight of diol and / or polyol, 0.4-1.6 parts by weight of active additive oligomer, 0.01-0.5 parts by weight of deionized water, 0.1-0.2 parts by weight of silicone surfactant, and 0.01-0.2 parts by weight of intermediate layer catalyst.

[0008] Preferably, the diisocyanate is one or a mixture of two of 1,6-hexamethylene diisocyanate, 2-methyl-1,5-pentamethylene diisocyanate, 2,4,4-trimethyl-hexamethylene diisocyanate, diphenylmethane diisocyanate and isophorone diisocyanate in any ratio.

[0009] Preferably: the active additive oligomer is a multipolymer of ethylene and methyl methacrylate or methyl acrylate having at least one active group, and a molecular weight of 500-2000; the active group is at least one of epoxy, isocyanate, silane coupling, sulfonic acid, amino and cyano.

[0010] Preferably: the silane coupling group is:

[0011]

[0012] Wherein, R1 and R2 are C1-C4 alkyl R or -OR respectively, and R3 is C1-C6 alkyl.

[0013] Preferably: the intermediate layer catalyst comprises triethylenediamine and a metal catalyst in a mass ratio of 1:1-2, and the metal catalyst is purchased from CUCAT-LCA, CUCAT-SW02D, BCAT-E20C, BCAT-T100R or ZCAT-T50 of Guangzhou Yourun Synthetic Materials Co., Ltd.

[0014] Preferably, the oligomer polyol is a polycarbonate polyol, polyoxypropylene glycol, polyether triol or polytetramethylene ether alcohol having a molecular weight of 1000-2800.

[0015] Preferably: the diol is ethylene glycol, propylene glycol, butylene glycol, neopentyl glycol or 1,6-hexanediol, the polyol is triethanolamine, glycerol or trimethylolpropane, and the silicone surfactant is ZX-101A, ZX-101B or ZX-X101 purchased from Laiyang Zhongxing Silicone Technology Co., Ltd.

[0016] Preferably: the aqueous polyurethane slurry includes 20-40 parts of diisocyanate, 40-60 parts of polyester polyol, 150-220 parts of deionized water, 0.4-2 parts of diol chain extender, 2-5 parts of triethylamine, 0.2-1 parts of thickener, 0.3-2 parts of foam stabilizer, 1-3 parts of cross-linking agent, 0.1-1 parts of leveling agent and 0.01-0.1 parts of aqueous catalyst, and chitosan accounting for 0.5-2% of the mass ratio of the aqueous polyurethane slurry, and the aqueous catalyst is ZCAT-T50.

[0017] Preferably: the diisocyanate is one or two of 1,6-hexamethylene diisocyanate, 2-methyl-1,5-pentamethylene diisocyanate, 2,4,4-trimethyl-hexamethylene diisocyanate, diphenylmethane diisocyanate and isophorone diisocyanate mixed in any ratio; the relative molecular mass of the polyester polyol is 1500-2500.

[0018] Preferably: the diol chain extender is ethylene glycol, propylene glycol, butanediol, neopentyl glycol or 1,6-hexanediol; the crosslinking agent is a polyisocyanate crosslinking agent; and the leveling agent is BYK-3565.

[0019] Through the above scheme, it can be known that the present application provides a highly peelable and hydrolysis-resistant water-based polyurethane synthetic leather, which is formed by coating a water-based polyurethane slurry containing chitosan on a release paper to form a film, so that the surface layer forms a bonding structure with the chitosan when the isocyanate dispersed component is coated, and thus the interfacial bonding force between the modified tackifying intermediate layer and the surface layer is significantly improved. At the same time, the active added oligomer has the effect of enhancing the activity of chitosan, thereby achieving the cross-linking bonding strength between the isocyanate dispersed component and the water-based polyurethane slurry, and based on the jungle test under constant temperature and humidity conditions of 70°C and 95%RH for 10 weeks, the peel strength retention rate is greater than 82%, and the dry peel strength is greater than 125N / 3cm. Performance test results achieve green environmental protection, energy saving and emission reduction, cost reduction, and significantly improve the peel strength and extend the service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying any creative work.

[0021] Figure 1 This is a schematic structural diagram of the highly peelable and hydrolysis-resistant water-based polyurethane synthetic leather disclosed in this application.

[0022] Explanation of reference numerals: 1. waterborne polyurethane pretreated base fabric; 2. modified adhesion-enhancing middle layer; 3. surface layer. DETAILED DESCRIPTION

[0023] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0024] It should be mentioned that the thickener was purchased from Guangdong Yongfeng Chemical Co., Ltd. and the crosslinker was purchased from Hefei Hengtian New Material Technology Co., Ltd. The solidification in the embodiment of the present application was carried out using a solidification liquid, and the thermal curing was carried out in an oven at 110-125°C for 1-4 minutes.

[0025] The highly peelable and hydrolysis-resistant water-based polyurethane synthetic leather of the present application will be specifically described below.

[0026] like Figure 1 As shown, a highly peelable and hydrolysis-resistant water-based polyurethane synthetic leather comprises a water-based polyurethane pre-treated base fabric, a modified tackifying intermediate layer and a surface layer. The surface layer is obtained by coating a water-based polyurethane slurry on a release paper and drying to form a film. The modified tackifying intermediate layer is formed by coating an isocyanate dispersed component on the surface of the surface layer, and after semi-curing treatment, it is bonded to the water-based polyurethane pre-treated base fabric and cross-linked and cured.

[0027] The waterborne polyurethane pre-treated base fabric is obtained by coating a slurry with a solid content of 30-50% or more of cationic waterborne polyurethane on a woven fabric, a non-woven fabric or a microfiber base fabric, and then solidifying or thermally curing the slurry. The slurry contains 0.2-2 parts of a silane coupling agent and 1-3 parts of a curing agent by mass. The curing agent is a waterborne isocyanate blocked curing agent 628.

[0028] It should be mentioned that the waterborne polyurethane slurry contains chitosan accounting for 0.5-2% by mass. Among them, the particle size of chitosan in the embodiment of the present application is 60-200nm, so as to be better dispersed in the waterborne polyurethane slurry, and then in the curing process, the surface hydroxyl and amino groups are used as active groups to enhance the bonding strength of the surface when it is bonded with the modified tackifying intermediate layer. At the same time, the isocyanate dispersing component includes 40-50 parts by weight of diisocyanate, 55-70 parts of oligomer polyols, 1-3 parts of diols and / or polyols, 0.4-1.6 parts of active additive oligomers, 0.01-0.5 parts of deionized water, 0.1-0.2 parts of silicone surfactants, and 0-0.2 parts of intermediate layer catalysts.

[0029] It should be noted that the diisocyanate in the examples of the present application is one or two of 1,6-hexamethylene diisocyanate, 2-methyl-1,5-pentamethylene diisocyanate, 2,4,4-trimethyl-hexamethylene diisocyanate, diphenylmethane diisocyanate and isophorone diisocyanate mixed in any ratio.

[0030] In the waterborne polyurethane slurry, the selected active additive oligomer is a multipolymer of ethylene and methyl methacrylate or methyl acrylate having at least one active group, and the molecular weight is 500-2000. Among them, the active group is at least one of epoxy group, isocyanate group, silane coupling group, sulfonic acid group, amino group and cyano group, and the two can be the same or different, but preferably at least one active group is a silane coupling group. And the silane coupling group should be as shown in the following formula:

[0031]

[0032] Wherein, R1 and R2 are C1-C4 alkyl R or -OR respectively, and R3 is C1-C6 alkyl.

[0033] At the same time, the intermediate layer catalyst includes triethylenediamine and a metal catalyst in a mass ratio of 1:1-2, and the metal catalyst is purchased from CUCAT-LCA, CUCAT-SW02D, BCAT-E20C, BCAT-T100R or ZCAT-T50 of Guangzhou Yourun Synthetic Materials Co., Ltd. The oligomer polyol is a polycarbonate polyol, polyoxypropylene glycol, polyether triol or polytetrahydrofuran ether alcohol with a molecular weight of 1000-2800. The diol is ethylene glycol, propylene glycol, butanediol, neopentyl glycol or 1,6-hexanediol, the polyol is triethanolamine, glycerol or trimethylolpropane, and the silicone surfactant is ZX-101A, ZX-101B or ZX-X101 purchased from Laiyang Zhongxing Silicone Technology Co., Ltd.

[0034] In order to maintain effective bonding strength of the surface layer in the process of forming a multi-layer structure synthetic leather through the modified tackifying intermediate layer and the waterborne polyurethane pretreated base fabric, the waterborne polyurethane slurry includes 20-40 parts of diisocyanate, 40-60 parts of polyester polyol, 150-220 parts of deionized water, 0.4-2 parts of diol chain extender, 2-5 parts of triethylamine, 0.2-1 parts of thickener, 0.3-2 parts of foam stabilizer, 1-3 parts of crosslinking agent, 0.1-1 parts of leveling agent and 0.01-0.1 parts of waterborne catalyst, and chitosan accounting for 0.5-2% of the mass ratio of the waterborne polyurethane slurry, and the waterborne catalyst is ZCAT-T50. The relative molecular mass of the polyester polyol is 1500-2500. The crosslinking agent is a polyisocyanate crosslinking agent. The leveling agent is BYK-3565. The foam stabilizer is DC-190. Of course, other foam stabilizers with corresponding effects can be used, which will not be described in detail here. The diol chain extender is ethylene glycol, propylene glycol, butanediol, neopentyl glycol or 1,6-hexanediol.

[0035] Embodiment 1

[0036] like Figure 1 As shown, a highly peelable and hydrolysis-resistant water-based polyurethane synthetic leather comprises a water-based polyurethane pre-treated base fabric, a modified tackifying intermediate layer and a surface layer. The surface layer is obtained by coating a water-based polyurethane slurry on a release paper and drying to form a film. The modified tackifying intermediate layer is formed by coating an isocyanate dispersed component on the surface of the surface layer, and after semi-curing treatment, it is bonded to the water-based polyurethane pre-treated base fabric and cross-linked and cured.

[0037] The waterborne polyurethane pre-treated base fabric is obtained by coating a woven fabric with a slurry of a cationic waterborne polyurethane solid content of 35% and solidifying the slurry, which contains 0.2 parts of a silane coupling agent and 1 part of a waterborne isocyanate blocked curing agent 628 by mass.

[0038] It should be mentioned that the water-based polyurethane slurry contains chitosan at a mass ratio of 0.5%. Among them, the particle size of chitosan in the embodiment of the present application is 60-200nm, so as to be better dispersed in the water-based polyurethane slurry, and then in the curing process, the surface hydroxyl and amino groups are used as active groups to enhance the bonding strength of the surface when it is bonded with the modified tackifying intermediate layer. At the same time, the isocyanate dispersing component includes 40 parts by weight of 1,6-hexamethylene diisocyanate, 55 parts of oligomer polyols, 1 part of ethylene glycol and triethanolamine in a mass ratio of 2:1, 0.4 parts of active additive oligomers, 0.01 parts of deionized water, 0.1 parts of silicone surfactants, and 0.01 parts of intermediate layer catalysts.

[0039] In the waterborne polyurethane slurry, the selected active additive oligomer is a multipolymer of ethylene and methyl methacrylate having at least one active group, and the molecular weight is 500-2000. Among them, the active groups are silane coupling groups and amino groups. And the silane coupling group should be as shown in the following formula:

[0040]

[0041] Wherein, R1 is methane, R2 is -OC 2 H 5 , R3 is n-pentyl.

[0042] At the same time, the intermediate layer catalyst includes triethylenediamine and a metal catalyst in a mass ratio of 1:1, and the metal catalyst is purchased from CUCAT-LCA of Guangzhou Yourun Synthetic Materials Co., Ltd. The oligomer polyol is a polycarbonate polyol with a molecular weight of 1000-2800. The silicone surfactant is ZX-X101 purchased from Laiyang Zhongxing Silicone Technology Co., Ltd.

[0043] In order to maintain effective bonding strength of the surface layer in the process of forming a multi-layer structure synthetic leather through the modified tackifying intermediate layer and the waterborne polyurethane pretreated base fabric, the waterborne polyurethane slurry includes 20 parts of 1,6-hexamethylene diisocyanate, 40 parts of polyester polyol, 150 parts of deionized water, 0.4 parts of diol chain extender, 2 parts of triethylamine, 0.2 parts of thickener, 0.3 parts of foam stabilizer, 1 part of polyisocyanate crosslinker, 0.1 parts of BYK-3565 and 0.01 parts of ZCAT-T50, and chitosan accounting for 0.5% of the mass ratio of the waterborne polyurethane slurry. Among them, the relative molecular mass of the polyester polyol is 1500-2500. The foam stabilizer is DC-190. Of course, other foam stabilizers with corresponding effects can be used, which will not be repeated here. The diol chain extender is ethylene glycol.

[0044] Embodiment 2

[0045] like Figure 1 As shown, a highly peelable and hydrolysis-resistant water-based polyurethane synthetic leather comprises a water-based polyurethane pre-treated base fabric, a modified tackifying intermediate layer and a surface layer. The surface layer is obtained by coating a water-based polyurethane slurry on a release paper and drying to form a film. The modified tackifying intermediate layer is formed by coating an isocyanate dispersed component on the surface of the surface layer, and after semi-curing treatment, it is bonded to the water-based polyurethane pre-treated base fabric and cross-linked and cured.

[0046] The waterborne polyurethane pre-treated base fabric is obtained by coating a woven fabric with a slurry of a cationic waterborne polyurethane solid content of 35% and solidifying the slurry, which contains 1 part of a silane coupling agent and 2 parts of a waterborne isocyanate blocked curing agent 628 in a mass ratio.

[0047] It should be mentioned that the waterborne polyurethane slurry contains chitosan accounting for 1% by weight. Among them, the particle size of the chitosan in the embodiment of the present application is 60-200nm, so as to be better dispersed in the waterborne polyurethane slurry, and then in the curing process, the surface hydroxyl and amino groups are used as active groups to enhance the bonding strength of the surface when it is bonded with the modified tackifying intermediate layer. At the same time, the isocyanate dispersing component includes 45 parts by weight of diphenylmethane diisocyanate, 62 parts of oligomer polyols, 2 parts of trimethylolpropane, 0.9 parts of active additive oligomers, 0.2 parts of deionized water, 0.15 parts of silicone surfactants, and 0.1 parts of intermediate layer catalysts.

[0048] In the waterborne polyurethane slurry, the selected active additive oligomer is a multipolymer of ethylene and methyl acrylate having at least one active group, and the molecular weight is 500-2000. Among them, the active groups in Example 2 of the present application are epoxy groups and silane coupling groups. And the silane coupling group should be as shown in the following formula:

[0049]

[0050] Wherein, R1 is ethyl, R2-O-CH 3 , R3 is butanyl.

[0051] Meanwhile, the intermediate layer catalyst includes triethylenediamine and a metal catalyst in a mass ratio of 1:1.5. The metal catalyst is purchased from ZCAT-T50 of Guangzhou Yourun Synthetic Materials Co., Ltd. The oligomer polyol is a polyether triol with a molecular weight of 1000-2800. The silicone surfactant is ZX-101A purchased from Laiyang Zhongxing Silicone Technology Co., Ltd.

[0052] In order to maintain effective bonding strength of the surface layer in the process of forming a multi-layer structure synthetic leather through the modified tackifying intermediate layer and the waterborne polyurethane pretreated base fabric, the waterborne polyurethane slurry includes 30 parts of diphenylmethane diisocyanate, 50 parts of polyester polyol, 190 parts of deionized water, 0.6 parts of diol chain extender, 3 parts of triethylamine, 0.75 parts of thickener, 1 part of foam stabilizer, 1.2 parts of polyisocyanate crosslinker, 0.3 parts of BYK-3565 and 0.05 parts of ZCAT-T50, and chitosan accounting for 1% of the mass ratio of the waterborne polyurethane slurry. The relative molecular mass of the polyester polyol is 1500-2500. The foam stabilizer is DC-190. Of course, other foam stabilizers with corresponding effects can be used, which will not be repeated here. The diol chain extender is butanediol.

[0053] Embodiment 3

[0054] like Figure 1As shown, a highly peelable and hydrolysis-resistant water-based polyurethane synthetic leather comprises a water-based polyurethane pre-treated base fabric, a modified tackifying intermediate layer and a surface layer. The surface layer is obtained by coating a water-based polyurethane slurry on a release paper and drying to form a film. The modified tackifying intermediate layer is formed by coating an isocyanate dispersed component on the surface of the surface layer, and after semi-curing treatment, it is bonded to the water-based polyurethane pre-treated base fabric and cross-linked and cured.

[0055] The waterborne polyurethane pre-treated base fabric is obtained by coating a microfiber base fabric with a slurry having a solid content of 50% of cationic waterborne polyurethane, and solidifying the slurry, which contains 2 parts of a silane coupling agent and 3 parts of a waterborne isocyanate blocked curing agent 628 in a mass ratio.

[0056] It should be mentioned that the water-based polyurethane slurry contains chitosan accounting for 2% by mass. Among them, the particle size of chitosan in the embodiment of the present application is 60-200nm, so as to be better dispersed in the water-based polyurethane slurry, and then in the curing process, the surface hydroxyl and amino groups are used as active groups to enhance the bonding strength of the surface when it is bonded with the modified tackifying intermediate layer. At the same time, the isocyanate dispersing component includes 50 parts by weight of 2-methyl-1,5-pentamethylene diisocyanate, 70 parts of oligomer polyols, 3 parts of 1,6-hexanediol and trimethylolpropane in a mass ratio of 1:1, 1.6 parts of active additive oligomers, 0.5 parts of deionized water, 0.2 parts of silicone surfactants, and 0.2 parts of intermediate layer catalysts.

[0057] In the waterborne polyurethane slurry, the selected active additive oligomer is a multipolymer of ethylene and methyl methacrylate having at least one active group and a molecular weight of 500-2000, wherein the active group is an amino group.

[0058] Meanwhile, the intermediate layer catalyst includes triethylenediamine and a metal catalyst in a mass ratio of 1:2. The metal catalyst is purchased from BCAT-E20C of Guangzhou Yourun Synthetic Materials Co., Ltd. The oligomer polyol is polytetrahydrofuran ether alcohol with a molecular weight of 1000-2800. The silicone surfactant is ZX-101B purchased from Laiyang Zhongxing Silicone Technology Co., Ltd.

[0059] In order to maintain effective bonding strength of the surface layer in the process of forming a multi-layer structure synthetic leather through the modified tackifying intermediate layer and the waterborne polyurethane pretreated base fabric, the waterborne polyurethane slurry includes 40 parts of 2-methyl-1,5-pentamethylene diisocyanate, 60 parts of polyester polyol, 220 parts of deionized water, 2 parts of 1,6-hexanediol, 5 parts of triethylamine, 1 part of thickener, 2 parts of foam stabilizer, 3 parts of polyisocyanate crosslinking agent, 1 part of BYK-3565 and 0.1 parts of ZCAT-T50, and chitosan accounting for 2% of the mass ratio of the waterborne polyurethane slurry. The relative molecular mass of the polyester polyol is 1500-2500. The foam stabilizer is DC-190. Of course, other foam stabilizers with corresponding effects can be used, which will not be repeated here.

[0060] Embodiment 4

[0061] The difference between Example 4 and Example 2 is that, in Example 4, the chitosan is soaked in an acid solution with a pH of 6.5-6.8 for 1-24 hours before use.

[0062] Comparative Example 1

[0063] The difference between Comparative Example 1 and Example 1 is that the active groups of the active additive oligomer in Comparative Example 1 are sulfonic acid groups and amino groups.

[0064] Comparative Example 2

[0065] The difference between Comparative Example 2 and Example 2 is that the aqueous polyurethane slurry in Comparative Example 2 contains chitosan in an amount of 0.1% by mass.

[0066] Comparative Example 3

[0067] The difference between Comparative Example 3 and Example 2 is that chitosan is not added to the aqueous polyurethane slurry in Comparative Example 3.

[0068] Comparative Example 4

[0069] The difference between Comparative Example 4 and Example 2 is that the particle size of chitosan in Comparative Example 4 is 20-40 nm.

[0070] Comparative Example 5

[0071] The difference between Comparative Example 5 and Example 2 is that no active additive oligomer is added in Comparative Example 5.

[0072] Performance Testing

[0073] Performance tests were conducted on Examples 1 to 4 and Comparative Examples 1 to 5, and the test contents and results are as follows:

[0074] 1. Hydrolysis resistance jungle test: Place the sample under constant temperature and humidity conditions of 70°C and 95% RH for 10 weeks and then test the peel strength retention rate;

[0075] 2. Peel strength test;

[0076] 3. Alkaline hydrolysis resistance test: soak the sample in 10% sodium hydroxide for 24 hours and then test the peel strength;

[0077] 4. Wear test: Based on Taber wear tester, H18 grinding wheel, 1Kg pressure and 2000R.

[0078] Table 1 Performance test results

[0079] Jungle Test Peel strength Alkali resistance test Wear test Embodiment 1 84% 137N / 3cm 120N / 3cm qualified Embodiment 2 85% 141N / 3cm 128N / 3cm qualified Embodiment 3 89% 155N / 3cm 140N / 3cm qualified Embodiment 4 87% 149N / 3cm 136N / 3cm qualified Comparative Example 1 82% 126N / 3cm 115N / 3cm qualified Comparative Example 2 75% 101N / 3cm 87N / 3cm qualified Comparative Example 3 67% 88N / 3cm 76N / 3cm Failure Comparative Example 4 80% 125N / 3cm 108N / 3cm qualified Comparative Example 5 81% 128N / 3cm 112N / 3cm qualified

[0080] It can be seen from the above table that the particle size of chitosan may increase its dispersion difficulty after reduction, and the force acting on the interfacial bonding force decreases, resulting in a decrease in peel strength; the active added oligomer and chitosan have a certain synergistic effect of improving the interfacial bonding force, so that in the preparation process of the high peeling hydrolysis-resistant water-based polyurethane synthetic leather, the active group is used to promote the interface combination, thereby effectively improving the peel strength between the interfaces and extending the service life of the high peeling hydrolysis-resistant water-based polyurethane synthetic leather. At the same time, based on comparative example 1 and embodiment 1, it can be found that when there is a silane coupling group in the active group, a certain degree of improvement in the interfacial bonding force will be achieved. Chitosan plays a key role in the interfacial bonding force in the embodiment of the present application, and a cross-linked structure is formed by chitosan and isocyanate dispersed components, thereby maintaining a high peel strength in the bonding structure, so as to effectively extend the service life.

[0081] In summary, the present application provides a highly peelable and hydrolysis-resistant water-based polyurethane synthetic leather, which is formed by coating a water-based polyurethane slurry containing chitosan on a release paper to form a film, so that the surface layer forms a bonding structure with the chitosan when the isocyanate dispersed component is coated, and thus the interfacial bonding force between the modified tackifying intermediate layer and the surface layer is significantly improved. At the same time, the active added oligomer has the effect of enhancing the activity of chitosan, thereby achieving the cross-linking bonding strength between the isocyanate dispersed component and the water-based polyurethane slurry, and based on the jungle test under constant temperature and humidity conditions of 70°C and 95%RH for 10 weeks, the peel strength retention rate is greater than 82%, and the dry peel strength is greater than 125N / 3cm. Performance test results achieve green environmental protection, energy saving and emission reduction, cost reduction, and significantly improve the peel strength and extend the service life.

[0082] The "first", "second", "third", "fourth", etc. (if any) referred to in this application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments described herein can be implemented in an order other than that illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, or devices.

[0083] It should be noted that the descriptions involving "first", "second", etc. in this application are only for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in this field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by this application.

[0084] Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for those skilled in the art, according to the idea of ​​the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A highly peelable and hydrolysis-resistant water-based polyurethane synthetic leather, Features: It includes a waterborne polyurethane pretreated base fabric, a modified tackifying intermediate layer and a surface layer; the surface layer is obtained by coating a waterborne polyurethane slurry on a release paper and drying to form a film; the modified tackifying intermediate layer is formed by coating an isocyanate dispersed component on the surface of the surface layer, and after semi-curing treatment, it is bonded to the waterborne polyurethane pretreated base fabric and cross-linked and cured; wherein, The aqueous polyurethane slurry contains chitosan in a mass ratio of 0.5-2%, and the particle size of the chitosan is 60-200nm; the isocyanate dispersing component includes 40-50 parts by weight of diisocyanate, 55-70 parts by weight of oligomer polyol, 1-3 parts by weight of diol and / or polyol, 0.4-1.6 parts by weight of active additive oligomer, 0.01-0.5 parts by weight of deionized water, 0.1-0.2 parts by weight of silicone surfactant, and 0.01-0.2 parts by weight of intermediate layer catalyst.

2. The highly peelable and hydrolysis-resistant water-based polyurethane synthetic leather according to claim 1, Features: The diisocyanate is one or two of 1,6-hexamethylene diisocyanate, 2-methyl-1,5-pentamethylene diisocyanate, 2,4,4-trimethyl-hexamethylene diisocyanate, diphenylmethane diisocyanate and isophorone diisocyanate mixed in any ratio.

3. The highly peelable and hydrolysis-resistant water-based polyurethane synthetic leather according to claim 1, Features: The active additive oligomer is a multipolymer of ethylene and methyl methacrylate or methyl acrylate having at least one active group and a molecular weight of 500-2000; the active group is at least one of epoxy, isocyanate, silane coupling, sulfonic acid, amino and cyano.

4. The highly peelable and hydrolysis-resistant water-based polyurethane synthetic leather according to claim 3, It is characterized in that The silane coupling group is: Wherein, R1 and R2 are C1-C4 alkyl R or -OR respectively, and R3 is C1-C6 alkyl.

5. The highly peelable and hydrolysis-resistant water-based polyurethane synthetic leather according to claim 1, Features: The intermediate layer catalyst includes triethylenediamine and a metal catalyst in a mass ratio of 1:1-2, and the metal catalyst is purchased from CUCAT-LCA, CUCAT-SW02D, BCAT-E20C, BCAT-T100R or ZCAT-T50 of Guangzhou Yourun Synthetic Materials Co., Ltd.

6. The highly peelable and hydrolysis-resistant water-based polyurethane synthetic leather according to claim 1, Features: The oligomer polyol is polycarbonate polyol, polyoxypropylene glycol, polyether triol or polytetrahydrofuran ether alcohol with a molecular weight of 1000-2800.

7. The highly peelable and hydrolysis-resistant water-based polyurethane synthetic leather according to claim 1, Features: The diol is ethylene glycol, propylene glycol, butylene glycol, neopentyl glycol or 1,6-hexanediol, the polyol is triethanolamine, glycerol or trimethylolpropane, and the silicone surfactant is ZX-101A, ZX-101B or ZX-X101 purchased from Laiyang Zhongxing Silicone Technology Co., Ltd.

8. The highly peelable and hydrolysis-resistant water-based polyurethane synthetic leather according to claim 1, Features: The waterborne polyurethane slurry comprises 20-40 parts of diisocyanate, 40-60 parts of polyester polyol, 150-220 parts of deionized water, 0.4-2 parts of diol chain extender, 2-5 parts of triethylamine, 0.2-1 parts of thickener, 0.3-2 parts of foam stabilizer, 1-3 parts of crosslinking agent, 0.1-1 parts of leveling agent and 0.01-0.1 parts of waterborne catalyst, and chitosan accounting for 0.5-2% by mass of the waterborne polyurethane slurry, wherein the waterborne catalyst is ZCAT-T50.

9. The highly peelable and hydrolysis-resistant water-based polyurethane synthetic leather according to claim 8, Features: The diisocyanate is one or two of 1,6-hexamethylene diisocyanate, 2-methyl-1,5-pentamethylene diisocyanate, 2,4,4-trimethyl-hexamethylene diisocyanate, diphenylmethane diisocyanate and isophorone diisocyanate mixed in any ratio; the relative molecular mass of the polyester polyol is 1500-2500.

10. The highly peelable and hydrolysis-resistant water-based polyurethane synthetic leather according to claim 8, Features: The diol chain extender is ethylene glycol, propylene glycol, butanediol, neopentyl glycol or 1,6-hexanediol; the crosslinking agent is a polyisocyanate crosslinking agent; and the leveling agent is BYK-3565.