Aramid insulation paper and preparation method and application thereof
By using potassium hydroxide and cationic polymer surfactant to reverse the fiber polarity during the preparation of aramid paper, the hollowing problem caused by the fiber electrostatic repulsion is solved, and the mechanical and insulating properties of aramid insulating paper are significantly improved. The performance gap between domestic products and foreign products has been narrowed.
Patent Information
- Application Number
- CN202411122145.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-15
AI Technical Summary
During the papermaking process, aramid paper paper is hollowed out due to the electrostatic repulsion of the settled fibers and chopped fibers, which affects the mechanical and insulating properties of the paper. The weak domestic technology accumulation leads to a gap in performance with foreign countries.
By adding aramid fibers to a mixed solution of dimethyl sulfoxide and water, potassium hydroxide is added to form a dispersion liquid, and then adding cationic polymer surfactant for polarity reversal, reducing the electrostatic repulsion between the fibers , improve the stability and performance of paper forming.
It significantly improves the mechanical and insulation performance of aramid insulating paper, reduces hollowing, improves the overall performance of paper, and achieves a performance level close to foreign products.
Smart Images

Figure CN118895683A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aramid paper, in particular to aramid insulating paper and a preparation method and application thereof. Background Art
[0002] Aramid paper is widely used in aerospace, rail transit, power equipment and other fields due to its excellent mechanical, insulation, heat resistance, corrosion resistance, flame retardancy and other properties. However, high-end aramid paper has been monopolized by companies such as DuPont in the United States and Teijin in Japan, resulting in high prices. Although some domestic manufacturers have achieved mass production of aramid paper, due to weak technical accumulation, some performance of the products is still lagging behind that of foreign countries. For aramid paper, since precipitated fibers and short-cut fibers are essentially two forms of the same substance, the surface electrical polarity of the two is the same, and there is electrostatic repulsion. During the papermaking process, the mutual repulsion between them hinders the stability of the interface, resulting in hollowing out of the paper after forming, which in turn affects the mechanical and insulation properties of the paper.
[0003] Therefore, an aramid insulation paper with excellent mechanical and insulating properties has broad application prospects. Summary of the invention
[0004] Based on this, the purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide an aramid insulation paper with excellent mechanical and insulation properties and a preparation method and application thereof.
[0005] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing aramid insulation paper, comprising the following steps:
[0006] (1) adding aramid short fibers or aramid fibrids to a mixed solution of dimethyl sulfoxide and water to obtain a mixed slurry, adding potassium hydroxide after ultrasonic stirring, and continuing ultrasonic stirring to obtain an aramid short fiber dispersion or an aramid fibrid dispersion;
[0007] (2) adding a cationic polymer surfactant to the aramid chopped fiber dispersion or the aramid fibrid dispersion, stirring evenly, filtering, washing, and drying to obtain reverse polarity aramid chopped fibers or reverse polarity aramid fibrids; the zeta potential of the reverse polarity aramid chopped fibers or reverse polarity aramid fibrids is 10 mV-45 mV; the cationic polymer surfactant is at least one of cationic polypropylene amine, polyquaternium salt polymer, and polyvinylamine; the polyquaternium salt polymer is at least one of polyquaternium-5, polyquaternium-6, polyquaternium-7, and polyquaternium-39;
[0008] (3) preparing a slurry suspension by dispersing the reverse polarity aramid chopped fibers and untreated aramid fibrils, and preparing the aramid insulation paper by dehydrating, forming and hot pressing the slurry suspension;
[0009] Alternatively, the reverse polarity aramid fibrids and untreated aramid chopped fibers are decomposed to form a slurry suspension, and the slurry suspension is dehydrated, formed, and heat-pressed to obtain the aramid insulation paper.
[0010] The inventors found in the actual experimental process that the outer molecular chain of aramid fiber is mainly composed of carbonyl groups. Due to its electronegativity, free electrons and hydroxyl groups in the environment will be adsorbed, showing negative polarity. When treated with a cationic polymer surfactant, the cationic components will be attracted by the negatively charged fibers and form a discrete layer on the surface of the negatively charged fibers. At this time, the electrical polarity of the fibers will be converted to positive, thereby generating electrostatic attraction between the fibers after polarity reversal and the untreated fibers. At the same time, the repulsion can still be maintained between the fibers after polarity reversal, thereby inhibiting the aggregation of fibers. The change in the electrical polarity of the fiber surface will be conducive to the uniform distribution of the fibers in the pulp and change the structure of the paper.
[0011] The inventors found in actual experimental processes that the potassium hydroxide (KOH) / dimethyl sulfoxide (DMSO) system was used to chemically swell and partially dissolve the aramid fibers, thereby enhancing the movement and diffusion capacity of the fiber molecular chains. The swollen or regenerated fibers shortened the distance between the aramid fibers and enhanced the interaction. At the same time, the inventors further found that the aramid fibers treated with the potassium hydroxide (KOH) / dimethyl sulfoxide (DMSO) system were more likely to achieve potential reversal in the subsequent mixing process with a cationic polymer surfactant. Furthermore, in the subsequent process of debonding and papermaking of reversed polarity aramid fibers and untreated aramid fibers, the prepared aramid insulating paper was more compact, significantly improving the mechanical properties and insulating properties of the aramid insulating paper.
[0012] The present invention starts from the perspective of the surface electrical polarity of the aramid fiber raw material, and through the means of polarity reversal, the polarity of one of the surfaces of the precipitated fibrils and the chopped fibers is reversed, thereby weakening the electrostatic repulsion between the interfaces of the precipitated fibrils and the chopped fibers, enhancing the stability of the paper interface, reducing the hollowing phenomenon, and further improving the mechanical and insulating properties of the paper.
[0013] Preferably, the aramid fiber raw material used in the present invention is para-aramid fiber or meta-aramid fiber. In the process of preparing aramid insulation paper, it can be para-aramid insulation paper or meta-aramid insulation paper.
[0014] Preferably, the aramid fiber raw material used in the present invention is meta-aramid fiber, and meta-aramid insulation paper is prepared.
[0015] Preferably, in step (1) and step (2), the aramid chopped fibers are processed to obtain reverse polarity aramid chopped fibers.
[0016] The inventors found in the actual experiment that due to the agglomeration of the original chopped fibers, the direct contact between different chopped fibers, and the rigidity of the chopped fibers themselves, the interface becomes difficult to relax. If the chopped fibers are polarity-reversed, the direct contact between the chopped fibers can be reduced. With less direct contact, the gaps between the chopped fibers are more likely to be surrounded by precipitated fibers, further reducing hollowing, thereby improving the mechanical and insulation properties of the finished paper.
[0017] Preferably, in step (1), the beating degree of the aramid chopped fiber slurry is 40-60°SR, and the beating degree of the aramid fibrid is 40-60°SR.
[0018] Preferably, the Zeta potential of the reverse polarity aramid chopped fibers or reverse polarity aramid fibrids is 29.5 mV-31.55 mV.
[0019] Preferably, in step (2), the cationic polymer surfactant is a mixture of cationic polypropylene amine, polyquaternary ammonium salt polymer and polyethylene amine.
[0020] Preferably, the weight ratio of the cationic polypropylene amine, the polyquaternary ammonium salt polymer and the polyvinyl amine is cationic polypropylene amine: polyquaternary ammonium salt polymer: polyvinyl amine = 1: (2-3): (1-2).
[0021] The inventors found in the actual experiment that the type of cationic polymer surfactant will further affect the Zeta potential, thereby further affecting the mechanical strength and insulation performance of the aramid insulation paper. When the cationic polymer surfactant is selected as above, the mechanical strength and insulation performance of the prepared aramid insulation paper are better.
[0022] Preferably, in the step (3), the absolute dry mass percentage of the reversed polarity aramid fibers and the untreated aramid fibers in the slurry suspension is 0.1-0.5wt%; the weight ratio of the reversed polarity aramid chopped fibers and the untreated aramid fibrils is reversed polarity aramid chopped fibers: untreated aramid fibrils = (1.5-2):1; the weight ratio of the reversed polarity aramid fibrils and the untreated aramid chopped fibers is reversed polarity aramid fibrils: untreated aramid chopped fibers = (1.5-2):1.
[0023] The inventors found in actual experiments that the weight ratio of the reversed polarity aramid fiber and the untreated aramid fiber will affect the mechanical strength and insulation performance of the aramid insulation paper finally prepared. When the weight ratio of the reversed polarity aramid fiber and the untreated aramid fiber is within the above range, the mechanical strength and insulation performance of the prepared aramid insulation paper are better.
[0024] Preferably, in step (1), the mass volume ratio of the aramid chopped fibers or aramid fibrids, dimethyl sulfoxide and water is aramid chopped fibers or aramid fibrids: dimethyl sulfoxide: water = (5-10): (500-1000): (10-30); the first ultrasonic stirring time is 10-30 min, the rotation speed is 1000-3000 r / min, the second ultrasonic stirring time is 12-24 h, the rotation speed is 1000-3000 r / min; the mass percentage of potassium hydroxide in the dispersion is 0.1-1.5%;
[0025] Preferably, in step (2), the mass percentage of the cationic polymer surfactant in the reverse polarity aramid chopped fibers or reverse polarity aramid fibrids is 0.2-1%.
[0026] Preferably, in the step (3), the rotation speed of the decomposition is 3000-5000 r / min, and the conditions of the hot pressing treatment are: the hot pressing temperature is 200-260° C., the hot pressing pressure is 8.0-10.0 MPa, and the hot pressing time is 10-30 min.
[0027] In addition, the present invention provides aramid insulation paper prepared by the preparation method of aramid insulation paper.
[0028] Furthermore, the present invention provides application of the aramid insulation paper in the field of transformers.
[0029] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention starts from the perspective of the surface electrical polarity of the aramid fiber raw material, and through the means of polarity reversal, the polarity of one of the surfaces of the precipitated fibers and the chopped fibers is reversed, thereby weakening the electrostatic repulsion between the interfaces of the precipitated fibers and the chopped fibers, enhancing the stability of the paper interface, reducing the hollowing phenomenon, and thereby improving the mechanical and insulating properties of the paper. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a cross-sectional view of the aramid insulation paper prepared in Example 1;
[0031] Figure 2 This is a cross-sectional view of the aramid insulation paper prepared in Comparative Example 1. DETAILED DESCRIPTION
[0032] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention will be further described below in conjunction with the accompanying drawings and specific embodiments. Its purpose is to understand the content of the present invention in detail, rather than to limit the present invention. All other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Unless otherwise specified, the experimental reagents and instruments designed for the implementation and comparative examples of the present invention are all commonly used ordinary reagents and instruments, which can be obtained from commercial channels. In the implementation and comparative examples, the experimental methods used are conventional methods unless otherwise specified; and unless otherwise specified, the raw materials used in parallel experiments are the same batch of raw materials.
[0033] Examples and Comparative Examples
[0034] A method for preparing aramid insulating paper comprises the following steps:
[0035] (1) adding aramid short fibers or aramid fibrids to a mixed solution of dimethyl sulfoxide and water to obtain a mixed slurry, adding potassium hydroxide after ultrasonic stirring, and continuing ultrasonic stirring to obtain an aramid short fiber dispersion or an aramid fibrid dispersion; the beating degree of the aramid short fiber slurry is 40-60°SR, and the beating degree of the aramid fibrids is 40-60°SR; the mass volume ratio of the aramid short fibers or aramid fibrids, dimethyl sulfoxide, and water is aramid short fibers or aramid fibrids: dimethyl sulfoxide: water = (5-10): (500-1000): (10-30); the first ultrasonic stirring time is 10-30 minutes, the rotation speed is 1000-3000 r / min, the second ultrasonic stirring time is 12-24 hours, and the rotation speed is 1000-3000 r / min; the mass percentage of the potassium hydroxide in the dispersion is 0.1-1.5%;
[0036] (2) adding a cationic polymer surfactant to the aramid chopped fibers dispersion or aramid fibrid dispersion, stirring evenly, filtering, washing, and drying to obtain reverse polarity aramid chopped fibers or reverse polarity aramid fibrids; the reverse polarity aramid chopped fibers or reverse polarity aramid fibrids have a Zeta potential of 10 mV-45 mV; the cationic polymer surfactant is at least one of cationic polypropylene amine, polyquaternium salt polymer, and polyvinyl amine; the polyquaternium salt polymer is at least one of polyquaternium-5, polyquaternium-6, polyquaternium-7, and polyquaternium-39; the mass percentage of the cationic polymer surfactant in the reverse polarity aramid chopped fibers or reverse polarity aramid fibrids is 0.2-1%;
[0037] (3) preparing a slurry suspension by dispersing the reverse polarity aramid chopped fibers and untreated aramid fibrils, and preparing the aramid insulation paper by dehydrating, forming and hot pressing the slurry suspension;
[0038] Or, the reverse polarity aramid fibrid and untreated aramid chopped fibers are decomposed to form a slurry suspension, and the slurry suspension is dehydrated, formed, and heat-pressed to obtain the aramid insulation paper;
[0039] The absolute dry mass percentage of the reversed polarity aramid fibers and the untreated aramid fibers in the slurry suspension is 0.1-0.5wt%; the weight ratio of the reversed polarity aramid chopped fibers and the untreated aramid fibrids is reversed polarity aramid chopped fibers: untreated aramid fibrids=(1.5-2):1; the weight ratio of the reversed polarity aramid fibrids and the untreated aramid chopped fibers is reversed polarity aramid fibrids: untreated aramid chopped fibers=(1.5-2):1;
[0040] The rotation speed of delamination is 3000-5000r / min, and the conditions of hot pressing treatment are: hot pressing temperature is 200-260°C, hot pressing pressure is 8.0-10.0MPa, and hot pressing time is 10-30min.
[0041] Preferably, the cationic polymer surfactant is a mixture of cationic polypropylene amine, polyquaternary ammonium salt polymer and polyvinyl amine, and the weight ratio of cationic polypropylene amine, polyquaternary ammonium salt polymer and polyvinyl amine is cationic polypropylene amine: polyquaternary ammonium salt polymer: polyvinyl amine = 1: (2-3): (1-2).
[0042] The aramid short fibers and aramid fibrids used in the examples and comparative examples of the present invention are all meta-aramid fibers.
[0043] Example 1
[0044] A method for preparing aramid insulating paper comprises the following steps:
[0045] (1) Aramid chopped fibers are added to a mixed solution of dimethyl sulfoxide and water to obtain a mixed slurry, and potassium hydroxide is added after ultrasonic stirring, and ultrasonic stirring is continued to obtain an aramid chopped fiber dispersion; the beating degree of the aramid chopped fiber slurry is 50°SR; the mass volume ratio of the aramid chopped fibers, dimethyl sulfoxide, and water is aramid chopped fibers: dimethyl sulfoxide: water = 8:800:20; the first ultrasonic stirring time is 10 minutes, the rotation speed is 3000 r / min, the second ultrasonic stirring time is 12 hours, and the rotation speed is 3000 r / min; the mass percentage of the potassium hydroxide in the dispersion is 0.6%;
[0046] (2) adding a cationic polymer surfactant to the aramid chopped fiber dispersion, stirring evenly, filtering, washing, and drying to obtain reverse polarity aramid chopped fibers; the cationic polymer surfactant is a mixture of cationic polyacrylamine, polyquaternary ammonium salt polymer, and polyvinylamine; the polyquaternary ammonium salt polymer is polyquaternium-5; the weight ratio is cationic polyacrylamine: polyquaternary ammonium salt polymer: polyvinylamine = 1:2:2; the mass percentage of the cationic polymer surfactant in the reverse polarity aramid chopped fibers is 0.4%;
[0047] (3) preparing a slurry suspension by dispersing the reverse polarity aramid chopped fibers and untreated aramid fibrils, and preparing the aramid insulation paper by dehydrating, forming and hot pressing the slurry suspension;
[0048] The absolute dry mass percentage of the reversed polarity aramid fibers and the untreated aramid fibers in the slurry suspension is 0.3wt%; the weight ratio of the reversed polarity aramid chopped fibers and the untreated aramid fibrils is reversed polarity aramid chopped fibers: untreated aramid fibrils = 1.5:1; the speed of debonding is 5000r / min, and the conditions of hot pressing treatment are: hot pressing temperature is 260°C, hot pressing pressure is 10.0MPa, and hot pressing time is 10min.
[0049] Example 2
[0050] A method for preparing aramid insulating paper comprises the following steps:
[0051] (1) Aramid chopped fibers are added to a mixed solution of dimethyl sulfoxide and water to obtain a mixed slurry, and potassium hydroxide is added after ultrasonic stirring, and ultrasonic stirring is continued to obtain an aramid chopped fiber dispersion; the beating degree of the aramid chopped fiber slurry is 40°SR; the mass volume ratio of the aramid chopped fibers, dimethyl sulfoxide, and water is aramid chopped fibers: dimethyl sulfoxide: water = 8:800:20; the first ultrasonic stirring time is 30 minutes, the speed is 1000 r / min, the second ultrasonic stirring time is 24 hours, the speed is 1000 r / min; the mass percentage of potassium hydroxide in the dispersion is 0.6%;
[0052] (2) adding a cationic polymer surfactant to the aramid chopped fiber dispersion, stirring evenly, filtering, washing, and drying to obtain reverse polarity aramid chopped fibers; the cationic polymer surfactant is a mixture of cationic polyacrylamine, polyquaternary ammonium salt polymer, and polyvinylamine; the polyquaternary ammonium salt polymer is polyquaternium-5; the weight ratio is cationic polyacrylamine: polyquaternary ammonium salt polymer: polyvinylamine = 1:2:2;
[0053] The mass percentage of the cationic polymer surfactant in the reverse polarity aramid short fibers is 0.4%;
[0054] (3) preparing a slurry suspension by dispersing the reverse polarity aramid chopped fibers and untreated aramid fibrils, and preparing the aramid insulation paper by dehydrating, forming and hot pressing the slurry suspension;
[0055] The absolute dry mass percentage of the reversed polarity aramid fibers and the untreated aramid fibers in the slurry suspension is 0.3wt%; the weight ratio of the reversed polarity aramid chopped fibers and the untreated aramid fibrils is reversed polarity aramid chopped fibers: untreated aramid fibrils = 1.5:1; the speed of debonding is 3000r / min, and the conditions of hot pressing treatment are: hot pressing temperature is 200°C, hot pressing pressure is 8.0MPa, and hot pressing time is 30min.
[0056] Example 3
[0057] A method for preparing aramid insulating paper comprises the following steps:
[0058] (1) adding aramid short fibers to a mixed solution of dimethyl sulfoxide and water to obtain a mixed slurry, adding potassium hydroxide after ultrasonic stirring, and continuing ultrasonic stirring to obtain an aramid short fiber dispersion; the beating degree of the aramid short fiber slurry is 60°SR; the mass volume ratio of the aramid short fibers, dimethyl sulfoxide, and water is aramid short fibers: dimethyl sulfoxide: water = 8:800:20; the first ultrasonic stirring time is 10-30 minutes, the speed is 2000 r / min, the second ultrasonic stirring time is 18 hours, the speed is 2000 r / min; the mass percentage of the potassium hydroxide in the dispersion is 0.6%;
[0059] (2) adding a cationic polymer surfactant to the aramid chopped fiber dispersion, stirring evenly, filtering, washing, and drying to obtain reverse polarity aramid chopped fibers; the cationic polymer surfactant is a mixture of cationic polyacrylamine, polyquaternary ammonium salt polymer, and polyvinylamine; the polyquaternary ammonium salt polymer is polyquaternium-5; the weight ratio is cationic polyacrylamine: polyquaternary ammonium salt polymer: polyvinylamine = 1:2:2;
[0060] The mass percentage of the cationic polymer surfactant in the reverse polarity aramid short fibers is 0.4%;
[0061] (3) preparing a slurry suspension by dispersing the reverse polarity aramid chopped fibers and untreated aramid fibrils, and preparing the aramid insulation paper by dehydrating, forming and hot pressing the slurry suspension;
[0062] The absolute dry mass percentage of the reversed polarity aramid fibers and the untreated aramid fibers in the slurry suspension is 0.3wt%; the weight ratio of the reversed polarity aramid chopped fibers and the untreated aramid fibrils is reversed polarity aramid chopped fibers: untreated aramid fibrils = 1.5:1; the speed of debonding is 4000r / min, and the conditions of hot pressing treatment are: hot pressing temperature is 230°C, hot pressing pressure is 9.0MPa, and hot pressing time is 20min.
[0063] Example 4
[0064] Compared with Example 1, only the cationic polymer surfactant in step (2) is different. Specifically, the cationic polymer surfactant is a mixture of cationic polyacrylamine, polyquaternium-5, and polyvinylamine; the polyquaternium polymer is polyquaternium-5; the weight ratio is cationic polyacrylamine: polyquaternium polymer: polyvinylamine = 1:3:1, and the remaining components, weight parts and preparation process are exactly the same as those in Example 1.
[0065] Example 5
[0066] Compared with Example 1, only the cationic polymer surfactant in step (2) is different. Specifically, the cationic polymer surfactant is a mixture of cationic polyacrylamine, polyquaternium-5, and polyvinylamine; the polyquaternium polymer is polyquaternium-5; the weight ratio is cationic polyacrylamine: polyquaternium polymer: polyvinylamine = 1:5:0.5, and the remaining components, weight parts and preparation process are exactly the same as those in Example 1.
[0067] Example 6
[0068] Compared with Example 1, only the cationic polymer surfactant in step (2) is different. Specifically, the cationic polymer surfactant is a mixture of cationic polyacrylamine, polyquaternium-5, and polyvinylamine; the polyquaternium polymer is polyquaternium-5; the weight ratio is cationic polyacrylamine: polyquaternium polymer: polyvinylamine = 3:1:1, and the remaining components, weight parts and preparation process are exactly the same as those in Example 1.
[0069] Example 7
[0070] Compared with Example 1, only the cationic polymer surfactant in step (2) is different. Specifically, the cationic polymer surfactant is cationic polypropylene amine. The remaining components, weight parts and preparation process are exactly the same as those in Example 1.
[0071] Example 8
[0072] Compared with Example 1, only the cationic polymer surfactant in step (2) is different. Specifically, the cationic polymer surfactant is polyquaternium-7. The remaining components, weight parts and preparation process are exactly the same as those in Example 1.
[0073] Example 9
[0074] Compared with Example 1, only the amount of cationic polymer surfactant in step (2) is different. Specifically, the mass percentage of the cationic polymer surfactant in the reverse polarity aramid short fibers is 0.3%. The remaining components, weight parts and preparation process are exactly the same as those in Example 1.
[0075] Example 10
[0076] Compared with Example 1, only the amount of cationic polymer surfactant in step (2) is different. Specifically, the mass percentage of the cationic polymer surfactant in the reverse polarity aramid short fibers is 1.3%. The remaining components, weight parts and preparation process are exactly the same as those in Example 1.
[0077] Embodiment 11
[0078] Compared with Example 1, only the amount of cationic polymer surfactant in step (2) is different. Specifically, the mass percentage of the cationic polymer surfactant in the reverse polarity aramid short fibers is 2%. The remaining components, weight parts and preparation process are exactly the same as those in Example 1.
[0079] Example 12
[0080] Compared with Example 1, only the amount of cationic polymer surfactant in step (2) is different. Specifically, the mass percentage of the cationic polymer surfactant in the reverse polarity aramid short fibers is 0.05%. The remaining components, weight parts and preparation process are exactly the same as those in Example 1.
[0081] Embodiment 13
[0082] Compared with Example 1, only the weight ratio of reverse polarity aramid chopped fibers and untreated aramid fibrids in step (3) is different, reverse polarity aramid chopped fibers: untreated aramid fibrids = 2:1, and the remaining components, weight parts and preparation process are exactly the same as those in Example 1.
[0083] Embodiment 14
[0084] Compared with Example 1, only the weight ratio of reversed polarity aramid chopped fibers and untreated aramid fibrids in step (3) is different, reversed polarity aramid chopped fibers: untreated aramid fibrids = 3:1, and the remaining components, weight parts and preparation process are exactly the same as those in Example 1.
[0085] Embodiment 15
[0086] Compared with Example 1, only the weight ratio of reversed polarity aramid chopped fibers and untreated aramid fibrids in step (3) is different, reversed polarity aramid chopped fibers: untreated aramid fibrids = 1:1, and the remaining components, weight parts and preparation process are exactly the same as those in Example 1.
[0087] Example 16
[0088] Compared with Example 1, only the reverse polarity aramid chopped fibers are changed to reverse polarity aramid fibrids, and the other components, weight parts and preparation process are exactly the same as those in Example 1.
[0089] Comparative Example 1
[0090] Compared with Example 1, the polarity reversal operation is not performed. Specifically, the preparation method of the aramid insulating paper is as follows:
[0091] (1) Aramid chopped fibers are added to a mixed solution of dimethyl sulfoxide and water to obtain a mixed slurry, and potassium hydroxide is added after ultrasonic stirring, and ultrasonic stirring is continued to obtain an aramid chopped fiber dispersion; the beating degree of the aramid chopped fiber slurry is 50°SR; the mass volume ratio of the aramid chopped fibers, dimethyl sulfoxide, and water is aramid chopped fibers: dimethyl sulfoxide: water = 8:800:20; the first ultrasonic stirring time is 10 minutes, the rotation speed is 3000 r / min, the second ultrasonic stirring time is 12 hours, and the rotation speed is 3000 r / min; the mass percentage of the potassium hydroxide in the dispersion is 0.6%;
[0092] (2) preparing a slurry suspension by dehydrating the aramid chopped fibers and aramid fibrils prepared in step (1), and performing a dehydration, forming, and hot pressing treatment on the slurry suspension to obtain the aramid insulating paper;
[0093] The absolute dry mass percentage of aramid fiber in the slurry suspension is 0.3wt%; the weight ratio of the aramid chopped fiber and the aramid precipitated fiber is aramid chopped fiber: aramid precipitated fiber = 1.5:1; the speed of debonding is 5000r / min, and the conditions of hot pressing treatment are: hot pressing temperature is 260°C, hot pressing pressure is 10.0MPa, and hot pressing time is 10min.
[0094] Performance Testing
[0095] The Zeta potential test was carried out in accordance with GB / T 24993-2010 “Determination of Zeta Potential in the Wet End of Papermaking”.
[0096] The Zeta potential of the untreated meta-aramid short fibers used in the present invention is -11.3 mV, and the Zeta potential of the untreated meta-aramid fibrids used in the present invention is -14.8 mV.
[0097] The Zeta potential of the reversed polarity aramid chopped fibers or reversed polarity aramid fibrids prepared through steps (1)-(2) in the embodiment of the present invention is shown in Table 1, and the Zeta potential of the aramid chopped fibers in Comparative Example 1 of the present invention is shown in Table 1.
[0098] The tensile strength, elongation at break and electrical strength were tested in accordance with GB / T 29627.2-2013 “Polyaramid fiberboard for electrical use Part 2: Test methods” and GB / T20629.3-2019 “Non-cellulose paper for electrical use Part 3: Unfilled polyaramid fiber paper”. The test results are shown in Table 2 below.
[0099] Table 1
[0100]
[0101] Table 2
[0102]
[0103]
[0104] It can be seen from the above table that reversing the polarity of one of the precipitated fibers and the chopped fibers can improve the mechanical (tensile strength, elongation at break) and insulating properties (electrical strength) of aramid paper to a certain extent.
[0105] Depend on Figure 1-2 By comparison, it can be seen that the cross section of the aramid paper in Example 1 is more compact and less hollow, while the cross section of the aramid paper in Comparative Example 1 has more hollows. This indicates that when the preparation process and conditions are the same, the structure of the aramid paper is more compact when the polarity of one of the precipitated fibers and the chopped fibers is reversed.
[0106] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing aramid insulation paper, It is characterized in that The following steps are involved: (1) adding aramid short fibers or aramid fibrids to a mixed solution of dimethyl sulfoxide and water to obtain a mixed slurry, adding potassium hydroxide after ultrasonic stirring, and continuing ultrasonic stirring to obtain an aramid short fiber dispersion or an aramid fibrid dispersion; (2) adding a cationic polymer surfactant to the aramid chopped fiber dispersion or the aramid fibrid dispersion, stirring evenly, filtering, washing, and drying to obtain reverse polarity aramid chopped fibers or reverse polarity aramid fibrids; the reverse polarity aramid chopped fibers or reverse polarity aramid fibrids have a Zeta potential of 10 mV-45 mV; the cationic polymer surfactant is at least one of cationic polypropylene amine, polyquaternium salt polymer, and polyvinylamine; the polyquaternium salt polymer is at least one of polyquaternium-5, polyquaternium-6, polyquaternium-7, and polyquaternium-39; (3) preparing a slurry suspension by dispersing the reverse polarity aramid chopped fibers and untreated aramid fibrils, and preparing the aramid insulation paper by dehydrating, forming and hot pressing the slurry suspension; Alternatively, the reverse polarity aramid fibrids and untreated aramid chopped fibers are decomposed to form a slurry suspension, and the slurry suspension is dehydrated, formed, and heat-pressed to obtain the aramid insulation paper.
2. The method for preparing aramid insulating paper according to claim 1, It is characterized in that In the step (1), the beating degree of the aramid chopped fiber slurry is 40-60°SR, and the beating degree of the aramid fibrid is 40-60°SR.
3. The method for preparing aramid insulating paper according to claim 1, It is characterized in that In the step (2), the cationic polymer surfactant is a mixture of cationic polypropylene amine, polyquaternary ammonium salt polymer and polyethylene amine.
4. The method for preparing aramid insulating paper according to claim 3, It is characterized in that In the step (2), the weight ratio of cationic polypropylene amine, polyquaternary ammonium salt polymer and polyvinyl amine is cationic polypropylene amine: polyquaternary ammonium salt polymer: polyvinyl amine = 1: (2-3): (1-2).
5. The method for preparing aramid insulating paper according to claim 1, It is characterized in that In the step (3), the absolute dry weight percentage of the reversed polarity aramid fibers and the untreated aramid fibers in the slurry suspension is 0.1-0.5wt%; The weight ratio of the reverse polarity aramid chopped fibers and the untreated aramid fibrils is reverse polarity aramid chopped fibers: untreated aramid fibrils = (1.5-2):1; the weight ratio of the reverse polarity aramid fibrils and the untreated aramid chopped fibers is reverse polarity aramid fibrils: untreated aramid chopped fibers = (1.5-2):
1.
6. The method for preparing aramid insulating paper according to claim 1, It is characterized in that In the step (1), the mass volume ratio of the aramid chopped fibers or aramid fibrids, dimethyl sulfoxide and water is aramid chopped fibers or aramid fibrids: dimethyl sulfoxide: water = (5-10): (500-1000): (10-30); the first ultrasonic stirring time is 10-30 minutes, the rotation speed is 1000-3000 r / min, the second ultrasonic stirring time is 12-24 hours, the rotation speed is 1000-3000 r / min; the mass percentage of the potassium hydroxide in the dispersion is 0.1-1.5%; And / or, in step (2), the mass percentage of the cationic polymer surfactant in the reverse polarity aramid chopped fibers or reverse polarity aramid fibrids is 0.2-1%; The volume weight ratio of the aramid short fiber dispersion or aramid fibrid dispersion and the cationic polymer surfactant is: aramid short fiber dispersion or aramid fibrid dispersion: cationic polymer surfactant = (500-1000) mL: (2-5) g; And / or, in the step (3), the rotation speed of the decomposition is 3000-5000 r / min, and the conditions of the hot pressing treatment are: the hot pressing temperature is 200-260°C, the hot pressing pressure is 8.0-10.0 MPa, and the hot pressing time is 10-30 min.
7. Aramid insulating paper prepared by the method for preparing aramid insulating paper according to any one of claims 1 to 6.
8. Use of the aramid insulation paper according to claim 7 in the field of transformers.
Citation Information
Patent Citations
Preparation method of regenerated aramid composite paper
CN109457533A
Para-aramid nanofiber mica paper and preparation method thereof
CN111472193A
Meta-aramid resin liquid, meta-aramid fiber, aramid product and preparation method of meta-aramid resin liquid
CN113072808A
High-efficiency dispersion method of aramid fiber
CN115787346A
Method for treating a fibre stock for making of paper, board or the like and product
WO2014072587A1