Paper-based microwave composite dielectric substrate and preparation method thereof
Through the wet papermaking and vacuum hot pressing process of the short fiber reinforced fluororesin substrate, the problem of poor dielectric performance and uniformity of the paper-based microwave composite dielectric substrate in the prior art is solved, and a low loss and high uniformity of the dielectric is achieved. Substrate, suitable for high frequency applications.
Patent Information
- Application Number
- CN202411190295.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-28
AI Technical Summary
The existing paper-based microwave composite dielectric substrates have poor dielectric properties and uniformity, complex preparation process and difficult to produce in large quantities and stable production. The dielectric loss factor is high and the relative dielectric constant is uneven, which affects high frequency performance.
The microwave composite media substrate of short fiber reinforced fluororesin is used to regulate the fiber-resin distribution through the combination of inorganic or organic chopped fibers and fluororesin, and the wet papermaking technology and vacuum hot pressing process, so as to regulate the fiber-resin distribution, avoid the introduction of impurities, and improve the media substrate. Thickness uniformity and dielectric properties.
It realizes low relative dielectric constant, low dielectric loss factor, excellent thickness uniformity and relative dielectric constant uniformity, suitable for RF, millimeter wave and terahertz frequency bands, high reliability and low water absorption rate, suitable for high-speed computers and Industrial equipment and other fields.
Smart Images

Figure BDA0005014920010000101 
Figure BDA0005014920010000111 
Figure BDA0005014920010000112
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of microwave composite dielectric substrates and relates to a paper-based microwave composite dielectric substrate and a preparation method thereof. Background Art
[0002] Microwave composite dielectric substrate, also known as high-frequency substrate material or high-frequency copper-clad laminate, is a basic electronic material used to prepare printed circuit boards (PCBs) and various RF / microwave functional components. It is widely used in commercial communications, integrated circuits, industrial equipment, aerospace and other fields. With the upgrading of modern electronic information technology requirements for data transmission rate and transmission flux, the operating frequency, rated power and integration of electronic equipment are constantly increasing. Therefore, microwave composite dielectric substrates with low relative dielectric constant, low dielectric loss factor and high dielectric structure consistency must be used to achieve low latency, low attenuation and high reliability of terminal applications.
[0003] The prior art usually adopts a composite method of fiber-reinforced polymer resin to prepare the above-mentioned dielectric substrate, which has the following problems: 1) The types of fiber raw materials used are relatively single, and there is a lack of innovative development and utilization of high-performance fibers; 2) The technical route for preparing prepregs is relatively single, generally firstly using wet forming technology to prepare fiber base paper, and then the fiber base paper is used to prepare prepregs by multiple impregnation / coating of resin, which has cumbersome process steps and low efficiency; 3) The fiber base paper described in 2) has extremely poor strength and is easy to break, so a certain adhesive spraying treatment is often used in the wet paper web forming stage. The adhesive can improve the strength of the fiber base paper, but this adhesive will reduce the porosity of the paper, directly affecting the amount of glue applied in the subsequent impregnation / coating and the introduction of impurities into the final dielectric substrate, which will seriously affect the dielectric properties of the dielectric substrate; 4) The fiber-resin distribution in the semi-cured sheet prepared by the wet molding process in the prior art is uneven, affecting the dielectric and thickness uniformity and high-frequency performance stability of the dielectric substrate; 5) The cold pressing and sintering preparation process will cause the dielectric substrate to have more pores and be less dense, with high water absorption and poor performance stability in actual use. Therefore, the vacuum hot pressing and sintering process is often used in this field to prepare a nearly completely dense dielectric substrate.
[0004] Therefore, the shortcomings of the existing technology reflected in the products are high dielectric loss factor, high relative dielectric constant, poor uniformity of relative dielectric constant, poor thickness uniformity, difficulty in continuous engineering preparation, etc. Summary of the invention
[0005] In view of the problems that the paper-based microwave composite dielectric substrate prepared by the prior art has poor dielectric properties and uniformity, a complex preparation process and cannot be prepared stably in large quantities, the present invention provides a paper-based microwave composite dielectric substrate and a preparation method thereof. The paper-based microwave composite dielectric substrate of the present invention has a low relative dielectric constant, a low dielectric loss factor, excellent thickness uniformity and excellent relative dielectric constant uniformity. The method of the present invention is more economical, convenient and can be scalable for mass production.
[0006] The technical solution adopted by the present invention is as follows:
[0007] In one aspect, the present invention provides a paper-based microwave composite dielectric substrate, which is a short fiber reinforced fluororesin microwave composite dielectric substrate, and is made of the following raw materials in terms of weight percentage:
[0008] Inorganic or organic chopped fibers: 0-12wt%;
[0009] Inorganic fiber cotton or organic fibrillation / fibrillation: 3-20wt%;
[0010] Fluororesin: 68-97wt%.
[0011] Preferably, the content of the inorganic or organic chopped fibers is 0-10wt%;
[0012] Preferably, the content of the inorganic fiber cotton or organic fibrillated / fibridized fiber is 3-17wt%;
[0013] Preferably, the content of the fluororesin is 80-97 wt %.
[0014] Preferably, the inorganic chopped fibers are selected from alkali-free, low dielectric, high silica, high strength, hollow glass chopped fibers, quartz chopped fibers, boron nitride chopped fibers, etc., and the organic chopped fibers are selected from aromatic polyamide chopped fibers (including para-aramid and meta-aramid chopped fibers), aromatic heterocyclic chopped fibers (including poly(p-phenylene benzobisoxazole) (PBO), polybenzimidazole, poly(phenylene pyridine diimidazole), aramid III, polyimide fibers), etc.
[0015] Preferably, the inorganic chopped fibers have an average diameter of less than 10 micrometers and a length of 1-9 millimeters.
[0016] Preferably, the inorganic chopped fibers have an average diameter of 3-6 microns and a length of 5-7 millimeters.
[0017] Preferably, the organic chopped fibers have an average diameter of less than 15 micrometers and a length of 1-9 millimeters.
[0018] Preferably, the organic chopped fibers have an average diameter of 12-14 microns and a length of 2-7 millimeters.
[0019] Preferably, the inorganic fiber cotton is selected from alkali-free, low dielectric, high silica, high strength glass wool fiber, quartz glass wool fiber, boron nitride cotton fiber, etc., and the organic fibrillation / fibrillation is selected from aromatic polyamide fibrillation / fibrillation (including para- and meta-aramid fibrillation / fibrillation), aromatic heterocyclic fibrillation / fibrillation (including poly(p-phenylene benzobisoxazole), polybenzimidazole, polyphenylene pyridine diimidazole, aramid III, polyimide fibrillation / fibrillation), etc.
[0020] Preferably, the average diameter of the inorganic fiber cotton is less than or equal to 3 microns.
[0021] Preferably, the organic fibrillated / precipitated fibers are organic chopped fibers prepared by mechanical beating or chemical precipitation to obtain fibers with a beating degree of 25-85° SR.
[0022] More preferably, the organic fibrillated / fibridized fibers are organic chopped fibers prepared by mechanical beating or chemical precipitation to obtain fibers with a beating degree of 30-80° SR.
[0023] More preferably, the organic fibrillated / fibridized fibers are organic chopped fibers prepared by mechanical beating or chemical precipitation to obtain fibers with a beating degree of 50-70° SR.
[0024] Preferably, the fluororesin is selected from polytetrafluoroethylene, polyvinylidene fluoride, polyperfluoroethylene propylene and the like, more preferably polytetrafluoroethylene resin.
[0025] Preferably, the fluororesin is in a granular form with an average particle size of 0.15-0.35 micrometers.
[0026] Preferably, the fluororesin is in the form of a fluororesin suspension, which is a suspension in which particulate fluororesin is uniformly dispersed in an aqueous medium.
[0027] Preferably, in the fluororesin suspension, the content of the particulate fluororesin is 25-62 wt % (eg 60 wt %).
[0028] The paper-based microwave composite dielectric material prepared by the present invention has the following characteristics:
[0029] 1) The relative dielectric constant is as low as 2.11, the dielectric loss factor is as low as 0.0006, and the relative dielectric constant range of 9 points within the 500×600mm format is less than or equal to 0.04, and the thickness range of 9 points within the 500×600mm format is less than 10 microns. It has excellent isotropy and can meet the needs of high-performance and high-reliability dielectric substrates for RF, millimeter wave and even terahertz frequency band applications to the greatest extent;
[0030] 2) It has excellent processability and usage characteristics under high humidity conditions, with a water absorption rate as low as 0.01%. It can withstand the corrosion of various commonly used acids, alkalis, and organic solutions in PCB processing and 260°C soldering processing, and keep the dielectric substrate from warping and performance from degradation;
[0031] 3) Low density, which can effectively reduce the overall mass of electronic systems and expand their functions in large-scale circuit design;
[0032] 4) The raw materials used in the paper-based microwave composite dielectric substrate of the present invention are wide in range and easy to obtain, and the preparation process is more efficient than the prior art, is environmentally friendly, and is easy to industrialize and mass produce.
[0033] The present invention aims at the actual performance requirements of dielectric substrate materials for applications in millimeter wave and even terahertz frequency bands. By optimizing organic / inorganic high-performance fibers and fluororesins, and using fiber compounding methods to regulate the comprehensive performance of dielectric substrate materials, the present invention innovatively adopts advanced wet papermaking technology to give the dielectric substrate fiber-resin distribution uniformity in the micro-nano scale range and random orientation distribution characteristics within the fiber plane, and greatly avoids the introduction of various impurities and additives. Therefore, the paper-based microwave dielectric substrate prepared by the present invention has low relative dielectric constant and low dielectric loss factor, excellent thickness uniformity, excellent relative dielectric constant uniformity, high isotropy, low water absorption, etc., and has good application prospects in high-frequency, high-speed, and high-reliability fields such as RF / millimeter wave / terahertz circuits, high-speed computers, consumer electronics, and industrial equipment.
[0034] In another aspect, the present invention provides a method for preparing a paper-based microwave composite dielectric substrate, the method comprising the following steps:
[0035] 1) Dispersing the inorganic or organic chopped fibers in deionized water to obtain a suspension in which the inorganic or organic chopped fibers are fully dispersed. If inorganic or organic chopped fibers are selected, this step is required; if inorganic or organic chopped fibers are not selected, this step is omitted;
[0036] 2) dispersing the inorganic fiber cotton or the organic fibrillated / precipitated fiber in deionized water to obtain a suspension in which the inorganic fiber cotton or the organic fibrillated / precipitated fiber is fully dispersed;
[0037] 3) mixing and stirring the fully dispersed suspension of inorganic or organic chopped fibers obtained in step 1) and the fully dispersed suspension of inorganic fiber cotton or organic fibrillated / precipitated fibers obtained in step 2) to obtain a mixed fiber suspension; if step 1) does not exist, this step is not required;
[0038] 4) adding a flocculant to the fluororesin suspension for flocculation to obtain a flocculated fluororesin slurry;
[0039] 5) adding the flocculated fluororesin slurry in step 4) to the fiber mixed suspension in step 3) (or if step 3 does not exist, adding it to the inorganic fiber cotton or organic fibrillated / decomposed fiber suspension in step 2) to obtain a mixed slurry;
[0040] 6) wet-making the mixed slurry in step 5) and drying it to obtain a paper-based prepreg;
[0041] 7) heat treating the paper-based prepreg obtained in step 6) at a high temperature;
[0042] 8) The paper-based prepreg obtained in step 7) is laminated in single or multiple sheets according to the required thickness, and finally the outermost single or double sides are covered with copper foil and vacuum hot pressed to prepare a paper-based microwave composite dielectric substrate.
[0043] Preferably, in step 1), the mass concentration of the suspension in which the inorganic or organic chopped fibers are fully dispersed is 0.01-1%.
[0044] Preferably, in step 1), the inorganic or organic chopped fibers are dispersed in deionized water and dispersed in a hydraulic pulper at a speed of 1000-15000 r / min for 1-30 min to obtain a suspension in which the inorganic or organic chopped fibers are fully dispersed.
[0045] Preferably, in step 2), the mass concentration of the inorganic fiber cotton or organic fibrillated / fibridized fully dispersed suspension is 0.01-1%.
[0046] Preferably, in step 2), the inorganic fiber cotton or organic fibrillated / fibrillated is dispersed in deionized water and dispersed in a hydraulic pulper at a speed of 1000-25000 r / min for 1-25 min to obtain a suspension in which the inorganic fiber cotton or organic fibrillated / fibrillated is fully dispersed.
[0047] Preferably, in step 4), the fluororesin suspension is formed by dispersing granular fluororesin in deionized water.
[0048] Preferably, in step 4), the mass fraction of the fluororesin suspension is 25-62%.
[0049] Preferably, in step 4), the fluororesin suspension is a polytetrafluoroethylene suspension with a mass fraction of 25-62%.
[0050] Preferably, the flocculant is selected from one or more of cationic branched starch, dopamine hydrochloride, chitosan, polyethylene oxide, polyethyleneimine, polyacrylamide, and natural polymer-acrylamide copolymer.
[0051] Preferably, in step 4), the amount of the flocculant used is 0.01 wt%-10 wt% of the absolute dry mass of the total raw materials.
[0052] Preferably, in step 6), the wet papermaking refers to dehydrating and forming the mixed slurry obtained in step 5) on the wire section of a paper machine, and then drying it to obtain a paper-based prepreg.
[0053] Preferably, the papermaking machine can be selected from oblique wire, cylinder wire, super cylinder wire, Fourdrinier wire, clamp wire, and top wire papermaking machines.
[0054] Preferably, the drying method may be one or a combination of heat conduction, heat convection, and heat radiation; the drying environment may be normal pressure or vacuum conditions.
[0055] Preferably, in step 7), the high temperature condition is 180-320° C., and the equipment used can be a high temperature blast / vacuum oven, a muffle furnace, a tubular furnace, etc., and the environmental atmosphere is not limited.
[0056] Preferably, in step 7), the heat treatment time is 2-6 hours.
[0057] Preferably, in step 8), the paper-based prepregs used in the multi-layer lamination can be of the same type, or multiple types of prepregs can be used for lamination.
[0058] Preferably, in step 8), the copper foil is one or a combination of two selected from electrolytic copper foil, reverse copper foil or rolled copper foil, and has a thickness of 9 μm to 70 μm.
[0059] Preferably, in step 8), the vacuum hot pressing conditions are pressure 2-8 MPa, temperature 365° C.-400° C., vacuum degree 0.04-0.1 MPa, and hot pressing time 2-8 hours.
[0060] Preferably, in step 8), the thickness of the paper-based microwave composite dielectric substrate is in the range of 0.05-10 mm.
[0061] Preferably, the paper-based microwave composite dielectric material prepared in step 8) can be directly used in the fields of processing single / double-sided flexible / rigid PCBs, multilayer boards and various microwave functional components.
[0062] Compared with the prior art, the preparation process of the present invention has the following advantages:
[0063] 1) It avoids the two-stage preparation route of first making short fibers into base paper and then impregnating the base paper with resin in the prior art. The technology has fast forming speed, high efficiency, high repeatability and reliability, and is conducive to large-scale industrial production;
[0064] 2) The fiber / resin mass ratio can be adjusted simply and quickly, thereby flexibly adjusting the comprehensive performance of the dielectric substrate, overcoming the disadvantage of the difficulty in regulating the amount of glue in the impregnation method;
[0065] 3) The fiber skeleton and resin matrix in the semi-cured sheet are formed simultaneously during the papermaking process. The fiber-resin microscopic distribution uniformity in the micro-nano scale range is better than that of the impregnation method, so the dielectric properties of the prepared paper-based microwave composite dielectric substrate are more excellent; at the same time, due to the steric effect of the resin particles during the molding process, a part of the fibers are distributed along the thickness direction of the paper, which is beneficial to reduce the Z-direction thermal expansion coefficient of the dielectric substrate and improve the isotropy of the dielectric substrate;
[0066] 4) There are many types and forms of fibers that can be used, the sources are abundant, and they are easy to obtain, and the comprehensive performance of the prepared dielectric substrate is more excellent. DETAILED DESCRIPTION
[0067] The present invention is further described below in conjunction with embodiments, which are as follows:
[0068] Example 1
[0069] Raw materials and their proportions:
[0070] Inorganic fiber wool: 5wt% quartz glass wool fiber, average diameter 3 microns;
[0071] Fluororesin: 95wt% polytetrafluoroethylene resin, in the form of a water-dispersed suspension: the mass fraction of polytetrafluoroethylene particles is 60%, and the average particle size is 0.25 microns.
[0072] 1) Dispersing quartz glass wool fibers in deionized water at a concentration of 0.08 wt %, fixing the speed of the hydraulic pulper at 8000 r / min, and dispersing for 15 min to obtain a quartz glass wool fiber suspension;
[0073] 2) adding 0.1% of the total dry weight of cationic branched starch to the polytetrafluoroethylene suspension for flocculation treatment, and then mixing evenly with the quartz glass wool fiber suspension in step 1) to obtain a mixed slurry;
[0074] 3) pumping the mixed slurry in step 2) to an inclined wire paper machine, and after being fully dispersed in a headbox, the slurry is dehydrated and formed in a forming wire section of the inclined wire paper machine to obtain a wet paper web, and then dried to obtain a paper-based prepreg;
[0075] 4) Treat the paper-based prepreg in an oven at 200-240°C for 4-6 hours;
[0076] 5) The semi-cured sheets in step 4) are laminated, and each surface is covered with an electrolytic copper foil, and the temperature and pressure are kept at 0.08 MPa, 380°C, and 2.5 MPa for 2.5 hours to obtain a paper-based microwave composite dielectric substrate.
[0077] Example 2
[0078] Raw materials and their proportions:
[0079] Inorganic chopped fibers: 8wt% quartz glass chopped fibers, average diameter 4-5 microns, average length 6mm;
[0080] Inorganic fiber wool: 3wt% alkali-free glass wool fiber, average diameter 2 microns;
[0081] Fluororesin: 89wt% polytetrafluoroethylene resin, in the form of a water-dispersed suspension: the mass fraction of polytetrafluoroethylene particles is 60%, and the average particle size is 0.25 microns.
[0082] Preparation process steps:
[0083] 1) Disperse quartz glass chopped fibers in deionized water at a concentration of 0.1 wt% and set the speed of the hydraulic pulper at 3000.
[0084] r / min, disintegrate for 5 min to obtain a dispersed suspension of quartz glass chopped fibers;
[0085] 2) dispersing the alkali-free glass wool fibers in deionized water at a concentration of 0.2 wt %, and dispersing the fibers at a fixed speed of 10,000 r / min for 6 minutes to obtain an alkali-free glass wool fiber suspension;
[0086] 3) mixing the quartz glass chopped fiber suspension in step 1) and the alkali-free glass wool fiber suspension in step 2) to obtain a fiber mixed suspension;
[0087] 4) adding 0.15% of the total dry weight of cationic branched starch to the polytetrafluoroethylene suspension for flocculation treatment, and then mixing evenly with the fiber suspension in step 3) to obtain a mixed slurry;
[0088] 5) pumping the mixed slurry in step 4) to an inclined wire paper machine, and after being fully dispersed in a headbox, the slurry is dehydrated and formed in a forming wire section of the inclined wire paper machine to obtain a wet paper web, and then dried to obtain a paper-based prepreg;
[0089] 4) Treat the paper-based prepreg in an oven at 200-240°C for 4-6 hours;
[0090] 5) The semi-cured sheets in step 4) are laminated, and each surface is covered with an electrolytic copper foil, and the temperature and pressure are kept at 0.08 MPa, 380°C, and 3 MPa for 3 hours to obtain a paper-based microwave composite dielectric substrate.
[0091] Example 3
[0092] Raw materials and their proportions:
[0093] Inorganic fiber cotton: 3wt% high silica glass wool fiber, average diameter 2 microns;
[0094] 14wt% quartz glass wool fibers, average diameter 3 microns;
[0095] Fluororesin: 83wt% polytetrafluoroethylene resin, in the form of a water-dispersed suspension: the mass fraction of polytetrafluoroethylene particles is 60wt%, and the average particle size is 0.18 microns.
[0096] Preparation process steps:
[0097] 1) High silica glass wool fibers and quartz glass wool fibers are dispersed in deionized water at a concentration of 0.1 wt%, and the hydraulic pulper is fixed at a speed of 15000 r / min for 10 min to obtain a glass wool fiber suspension;
[0098] 2) adding 0.06% of the total dry weight of cationic branched starch to the polytetrafluoroethylene suspension for flocculation treatment, and then mixing evenly with the fiber mixed suspension in step 1) to obtain a mixed slurry;
[0099] 3) pumping the mixed slurry in step 2) to an inclined wire paper machine, and after being fully dispersed in a headbox, the slurry is dehydrated and formed in a forming wire section of the inclined wire paper machine to obtain a wet paper web, and then dried to obtain a paper-based prepreg;
[0100] 4) Treat the paper-based prepreg in an oven at 200-240°C for 4-6 hours;
[0101] 5) The semi-cured sheets in step 4) are laminated, and each surface is covered with an electrolytic copper foil, and the temperature and pressure are kept at 0.08 MPa, 385°C, and 4.5 MPa for 2 hours to obtain a paper-based microwave composite dielectric substrate.
[0102] Example 4
[0103] Raw materials and their proportions:
[0104] Organic fibrillation / fibridization: 3wt% poly(p-phenylene benzobisoxazole) fibrillated fiber, prepared by mechanical refining, beating degree 65°SR;
[0105] Fluororesin: 97wt% polytetrafluoroethylene resin, in the form of water-dispersed suspension: the mass fraction of polytetrafluoroethylene particles is 60wt%, and the average particle size is 0.3 microns.
[0106] Preparation process steps:
[0107] 1) PBO fibrillated fibers were dispersed in deionized water at a concentration of 0.3 wt%, and the speed of the hydraulic pulper was fixed at 6000 r / min for 6 minutes to obtain a PBO fibrillated fiber suspension;
[0108] 2) adding polyethyleneimine in an amount of 0.1% by absolute dry weight of the total raw materials to the polytetrafluoroethylene suspension for flocculation treatment, and then mixing evenly with the PBO fibrillated fiber suspension in step 1) to obtain a mixed slurry;
[0109] 3) pumping the mixed slurry in step 2) to an inclined wire paper machine, and after being fully dispersed in a headbox, the slurry is dehydrated in a wire section of the paper machine to obtain a wet paper web, and then dried to obtain a paper-based prepreg;
[0110] 4) Treat the paper-based prepreg in an oven at 240-260°C for 2-4 hours;
[0111] 5) The semi-cured sheets in 4) are laminated, and a rolled copper foil is covered on each surface. The paper-based microwave composite dielectric substrate is obtained by maintaining the temperature and pressure at a vacuum degree of 0.08 MPa, a temperature of 375° C., and a pressure of 4 MPa for 4 hours.
[0112] Example 5
[0113] Raw materials and their proportions:
[0114] Organic chopped fibers: 6wt% poly(p-phenylene benzobisoxazole) chopped fibers, average diameter 13 microns, average length 6 mm;
[0115] Organic fibrillation / fibridization: 4wt% poly(p-phenylene benzobisoxazole) fibrillated fiber, prepared by mechanical refining, beating degree 55°SR;
[0116] Fluororesin: 90wt% polytetrafluoroethylene resin, in the form of water-dispersed suspension: the mass fraction of polytetrafluoroethylene particles is 60wt%, and the average particle size is 0.3 microns.
[0117] Preparation process steps:
[0118] 1) PBO chopped fibers were dispersed in deionized water at a concentration of 0.05 wt%, and the speed of the hydraulic pulper was fixed at 3000 r / min for 1 min to obtain a PBO chopped fiber suspension;
[0119] 2) PBO fibrillated fibers were dispersed in deionized water at a concentration of 0.3 wt %, and the speed of the hydraulic pulper was fixed at 6000 r / min for 6 min to obtain a PBO fibrillated fiber suspension;
[0120] 3) mixing the PBO chopped fiber suspension of step 1) and the PBO fibrillated fiber suspension of step 2) to obtain a mixed fiber suspension;
[0121] 4) flocculating the polytetrafluoroethylene suspension with 0.06% of the total raw material absolute dry weight of polyethyleneimine, and then mixing it evenly with the fiber mixed suspension in step 3) to obtain a mixed slurry;
[0122] 5) pumping the mixed slurry in step 4) to a rotary screen paper machine, dehydrating the slurry to obtain a wet paper web, and then drying the wet paper web to obtain a paper-based prepreg;
[0123] 6) Treat the paper-based prepreg in an oven at 240-260°C for 2-4 hours;
[0124] 7) The semi-cured sheets in 6) are laminated, and a rolled copper foil is covered on each surface. The paper-based microwave composite dielectric substrate is obtained by maintaining the temperature and pressure at a vacuum degree of 0.08 MPa, a temperature of 370° C., and a pressure of 3.5 MPa for 3 hours.
[0125] Example 6
[0126] Raw materials and their proportions:
[0127] Organic chopped fibers: 3wt% poly(p-phenylene benzobisoxazole) chopped fibers, average diameter 13 microns, average length 6 mm;
[0128] Inorganic fiber wool: 8wt% alkali-free glass wool fiber, average diameter 2 microns;
[0129] Fluororesin: 89wt% polytetrafluoroethylene resin, in the form of a water-dispersed suspension: the mass fraction of polytetrafluoroethylene particles is 60wt%, and the average particle size is 0.22 microns.
[0130] Preparation process steps:
[0131] 1) PBO chopped fibers were dispersed in deionized water at a concentration of 0.05 wt%, and the speed of the hydraulic pulper was fixed at 3000 r / min for 3 minutes to obtain a PBO chopped fiber suspension;
[0132] 2) dispersing the alkali-free glass wool fibers in deionized water at a concentration of 0.2 wt %, and dispersing the fibers at a fixed speed of 10,000 r / min for 6 minutes to obtain an alkali-free glass wool fiber suspension;
[0133] 3) mixing the PBO chopped fiber suspension of step 1) and the alkali-free glass wool fiber suspension of step 2) to obtain a fiber mixed suspension;
[0134] 4) adding 0.06% of the total raw material absolute dry weight of polyethyleneimine to the polytetrafluoroethylene suspension for flocculation treatment, and then mixing evenly with the fiber mixed suspension in step 3) to obtain a mixed slurry;
[0135] 5) pumping the mixed slurry in step 4) to a rotary screen paper machine, dehydrating the slurry to obtain a wet paper web, and then drying the wet paper web to obtain a paper-based prepreg;
[0136] 6) Treat the paper-based prepreg in an oven at 230-260°C for 3-4 hours to fully remove organic impurities;
[0137] 7) The semi-cured sheets in 6) are laminated, and each surface is covered with an electrolytic copper foil, and the heat and pressure are maintained at a vacuum degree of 0.08 MPa, a temperature of 380° C., and a pressure of 3.5 MPa for 2 hours to obtain a paper-based microwave composite dielectric substrate.
[0138] Example 7
[0139] Raw materials and their proportions:
[0140] Organic chopped fibers: 10wt% poly(p-phenylene benzobisoxazole) chopped fibers, average diameter 13 microns, average length 3 mm;
[0141] Organic fibrillation / fibridization: 10wt% poly(p-phenylene benzobisoxazole) fibrillated fiber, prepared by mechanical refining, beating degree 35°SR;
[0142] Fluororesin: 80wt% polytetrafluoroethylene resin, in the form of a water-dispersed suspension: the mass fraction of polytetrafluoroethylene particles is 60wt%, and the average particle size is 0.28 microns.
[0143] The preparation process steps are the same as those in Example 5.
[0144] The performance test results of the paper-based microwave composite dielectric substrate of Examples 1-7 are shown in the following table:
[0145]
[0146] Note: The smaller the relative dielectric constant, the faster the signal transmission speed; the smaller the dielectric loss factor, the smaller the signal transmission loss.
[0147] Comparative Example 1: Preparation of paper-based microwave composite dielectric substrate by conventional impregnation method
[0148] Raw materials and their proportions:
[0149] Organic fibrillation / fibridization: poly(p-phenylene benzobisoxazole) fibrillated fiber, prepared by mechanical refining, beating degree 65°SR;
[0150] Fluororesin: polytetrafluoroethylene resin, in the form of water-dispersed suspension: the mass fraction of polytetrafluoroethylene particles is 60wt%, and the average particle size is 0.3 microns.
[0151] Preparation process steps:
[0152] 1) PBO fibrillated fibers were dispersed in deionized water at a concentration of 0.3 wt%, and the hydraulic pulper was set at a speed of 6000 r / min for 6 min to obtain a PBO fibrillated fiber suspension.
[0153] 2) The PBO fibrillated fiber suspension in step 1) is subjected to wet papermaking and drying to obtain fiber base paper.
[0154] 3) The fiber base paper is impregnated with a polytetrafluoroethylene emulsion with a solid content of 60 wt % by using a standard impregnation process in the prior art, and dried to obtain a paper-based prepreg.
[0155] 4) Treat the paper-based prepreg in an oven at 240-260°C for 2-4 hours;
[0156] 5) The semi-cured sheets in 4) are laminated, and then the two surfaces are covered with a rolled copper foil respectively, and the temperature and pressure are kept at 0.08 MPa, 375°C, and 4 MPa for 4 hours to obtain a paper-based microwave composite dielectric substrate.
[0157] The performance test results of the paper-based microwave composite dielectric substrate prepared in Comparative Example 1 are as follows:
[0158]
[0159] The dielectric properties of the paper-based microwave composite dielectric substrate prepared by the present invention are better than those of Comparative Example 1.
[0160] Comparative Example 2: Fiber Type Exploration Experiment
[0161] Raw materials and their proportions:
[0162] Inorganic fiber cotton: 5wt% alumina cotton fiber, average diameter 3 microns;
[0163] Fluororesin: 95wt% polytetrafluoroethylene resin, in the form of a water-dispersed suspension: the mass fraction of polytetrafluoroethylene particles is 60wt%, and the average particle size is 0.25 micrometer.
[0164] The preparation process steps are the same as in Example 1.
[0165] The performance test results of the paper-based microwave composite dielectric substrate prepared in Comparative Example 2 are as follows:
[0166]
[0167]
[0168] The performance of the paper-based microwave composite dielectric substrate prepared by the present invention is better than that of Comparative Example 2.
[0169] Comparative Example 3: Experimental study on fiber length
[0170] Raw materials and their proportions:
[0171] Organic chopped fibers: 6wt% poly(p-phenylene benzobisoxazole) chopped fibers, average diameter 13 microns, average length 12 mm;
[0172] Organic fibrillation / fibridization: 4wt% poly(p-phenylene benzobisoxazole) fibrillated fiber, prepared by mechanical refining, beating degree 55°SR;
[0173] Fluororesin: 90wt% polytetrafluoroethylene resin, in the form of water-dispersed suspension: the mass fraction of polytetrafluoroethylene particles is 60%, and the average particle size is 0.3 microns.
[0174] The preparation process steps are the same as those in Example 5.
[0175] Results: In Example 5, the chopped fibers were well dispersed and uniform, and the paper-based prepreg was of excellent quality. In Comparative Example 3, during the wet papermaking process, the PBO chopped fibers were severely flocculated, and the paper-based prepreg was poorly uniform. The performance test results of the paper-based microwave composite dielectric substrate prepared in Comparative Example 3 are shown in the following table.
[0176]
[0177] The dielectric properties of the paper-based microwave composite dielectric substrate prepared by the present invention are better than those of Comparative Example 3.
[0178] It can be seen from the above implementation and comparative examples that the dielectric loss factor of the dielectric substrate prepared by the present invention is as low as 0.0006, which belongs to the ultra-low loss range, and is 30-40% lower than the dielectric loss factor of the prior art, which is significantly improved; the relative dielectric constant reaches or exceeds the prior art, and has a more excellent relative dielectric constant and thickness uniformity, which can significantly improve the signal transmission speed and antenna radiation efficiency; at the same time, the extremely low water absorption rate and low density reach or exceed the existing technical level, which improves the manufacturing technology and comprehensive performance level of the existing paper-based microwave composite dielectric substrate as a whole, and has important practical application value.
Claims
1. A paper-based microwave composite dielectric substrate, made of the following raw materials in parts by weight: Inorganic or organic chopped fibers: 0-12wt%; Inorganic fiber cotton or organic fibrillation / fibrillation: 3-20wt%; Fluororesin: 68-97wt%.
2. The paper-based microwave composite dielectric substrate according to claim 1, wherein: The content of the inorganic or organic chopped fibers is 0-10wt%; Preferably, the content of the inorganic fiber cotton or organic fibrillated / fibridized fiber is 3-17wt%; Preferably, the content of the fluororesin is 80-97wt%; Preferably, the inorganic or organic chopped fibers are selected from alkali-free, low dielectric, high silica, high strength, hollow glass chopped fibers, quartz chopped fibers, boron nitride chopped fibers, etc., and the organic chopped fibers are selected from aromatic polyamide chopped fibers (including para-aramid chopped fibers and meta-aramid chopped fibers), aromatic heterocyclic chopped fibers (including poly(p-phenylene benzobisoxazole), polybenzimidazole, poly(phenylene pyridine diimidazole), aramid III, polyimide fibers, etc.; Preferably, the inorganic chopped fibers have an average diameter of less than 10 microns and a length of 1-9 millimeters; Preferably, the inorganic chopped fibers have an average diameter of 3-6 microns and a length of 5-7 millimeters; Preferably, the organic chopped fibers have an average diameter of less than 15 microns and a length of 1-9 millimeters; Preferably, the organic chopped fibers have an average diameter of 12-14 microns and a length of 2-7 millimeters.
3. The paper-based microwave composite dielectric substrate according to claim 1 or 2, wherein: The inorganic fiber cotton is selected from alkali-free, low dielectric, high silica, high strength glass wool fiber, quartz glass wool fiber, boron nitride cotton fiber, etc., and the organic fibrillation / fibrid is selected from aromatic polyamide fibrillation / fibrid (including para- and meta-aramid fibrillation / fibrid), aromatic heterocyclic fibrillation / fibrid (including poly(p-phenylene benzobisoxazole), polybenzimidazole, poly(phenylene pyridine diimidazole), aramid III, polyimide fibrillation / fibrid), etc.; Preferably, the average diameter of the inorganic fiber cotton is less than or equal to 3 microns; Preferably, the organic fibrillated / precipitated fibers are organic chopped fibers prepared by mechanical beating or chemical precipitation to obtain a beating degree of 25-85° SR; Preferably, the organic fibrillated / precipitated fibers are organic chopped fibers prepared by mechanical beating or chemical precipitation to obtain a beating degree of 30-80° SR; More preferably, the organic fibrillated / fibridized fibers are organic chopped fibers prepared by mechanical beating or chemical precipitation to obtain fibers with a beating degree of 50-70° SR.
4. The paper-based microwave composite dielectric substrate according to any one of claims 1 to 3, wherein: The fluororesin is selected from polytetrafluoroethylene, polyvinylidene fluoride, polyperfluoroethylene propylene and the like, more preferably polytetrafluoroethylene resin; Preferably, the fluororesin is in granular form with an average particle size of 0.15-0.35 micrometers; Preferably, the fluororesin is in the form of a fluororesin suspension, which is a suspension formed by uniformly dispersing granular fluororesin in an aqueous medium; Preferably, in the fluororesin suspension, the content of the granular fluororesin is 25-62 wt %.
5. A method for preparing the paper-based microwave composite dielectric substrate according to any one of claims 1 to 4, the method comprising the following steps: 1) dispersing the inorganic or organic chopped fibers in deionized water to obtain a suspension in which the inorganic or organic chopped fibers are fully dispersed; 2) dispersing the inorganic fiber cotton or the organic fibrillated / precipitated fiber in deionized water to obtain a suspension in which the inorganic fiber cotton or the organic fibrillated / precipitated fiber is fully dispersed; 3) mixing and stirring the fully dispersed suspension of inorganic or organic chopped fibers obtained in step 1) and the fully dispersed suspension of inorganic fiber cotton or organic fibrillated / precipitated fibers obtained in step 2) to obtain a mixed fiber suspension; If step 1) does not exist, this step is not required; 4) adding a flocculant to the fluororesin suspension for flocculation to obtain a flocculated fluororesin slurry; 5) adding the flocculated fluororesin slurry in step 4) to the fiber mixed suspension in step 3) (or if step 3 does not exist, adding it to the inorganic fiber cotton or organic fibrillated / decomposed fiber suspension in step 2) to obtain a mixed slurry; 6) wet-making the mixed slurry in step 5) and drying it to obtain a paper-based prepreg; 7) heat treating the paper-based prepreg obtained in step 6) at a high temperature; 8) The paper-based prepreg obtained in step 7) is laminated in single or multiple sheets according to the required thickness, and finally the outermost single or double sides are covered with copper foil and vacuum hot pressed to prepare a paper-based microwave composite dielectric substrate.
6. The method according to claim 5, wherein: In step 1), the mass concentration of the suspension in which the inorganic or organic chopped fibers are fully dispersed is 0.01-1%; Preferably, in step 1), the inorganic or organic chopped fibers are dispersed in deionized water and dispersed in a hydraulic pulper at a speed of 1000-15000 r / min for 1-30 min to obtain a suspension in which the inorganic or organic chopped fibers are fully dispersed.
7. The method according to claim 5 or 6, wherein: In step 2), the mass concentration of the inorganic fiber cotton or organic fibrillated / fibridized fully dispersed suspension is 0.01-1%; Preferably, in step 2), the inorganic fiber cotton or organic fibrillated / fibrillated is dispersed in deionized water and dispersed in a hydraulic pulper at a speed of 1000-25000 r / min for 1-25 min to obtain a suspension in which the inorganic fiber cotton or organic fibrillated / fibrillated is fully dispersed.
8. The method according to any one of claims 5 to 7, wherein: In step 4), the fluororesin suspension is formed by dispersing granular fluororesin in deionized water; Preferably, in step 4), the mass fraction of the fluororesin suspension is 25-62%; Preferably, in step 4), the fluororesin suspension is a polytetrafluoroethylene suspension with a mass fraction of 25-62%; Preferably, the flocculant is selected from one or more of cationic branched starch, dopamine hydrochloride, chitosan, polyethylene oxide, polyethyleneimine, polyacrylamide, and natural polymer-acrylamide copolymer; Preferably, in step 4), the amount of the flocculant used is 0.01 wt%-10 wt% of the absolute dry mass of the total raw materials.
9. The method according to any one of claims 5 to 8, wherein: In step 6), the wet papermaking refers to dehydrating the mixed slurry obtained in step 5) on the wire section of a paper machine to obtain a wet paper web, and then drying it to obtain a paper-based prepreg; Preferably, the papermaking machine can be selected from oblique wire, cylinder wire, super cylinder wire, Fourdrinier wire, clamp wire, and top wire papermaking machines; Preferably, the drying method may be one or a combination of heat conduction, heat convection, and heat radiation; the drying environment may be normal pressure or vacuum conditions.
10. The method according to any one of claims 5 to 9, wherein: In step 7), the high temperature condition is 180-320° C., and the equipment used can be a high temperature blast / vacuum oven, a muffle furnace, or a tubular furnace; Preferably, in step 7), the heat treatment time is 2-6 hours; Preferably, in step 8), the paper-based prepregs used in the multi-layer lamination can be of the same type, or multiple types of prepregs can be used for lamination; Preferably, in step 8), the copper foil is one or a combination of electrolytic copper foil, reverse copper foil or rolled copper foil, and has a thickness of 9 μm to 70 μm; Preferably, in step 8), the vacuum hot pressing conditions are pressure 2-8 MPa, temperature 365° C.-400° C., vacuum degree 0.04-0.1 MPa, and hot pressing time 2-8 hours; Preferably, in step 8), the thickness of the paper-based microwave composite dielectric substrate is in the range of 0.05-10 mm.
Citation Information
Patent Citations
Composite material and sheet for microwave circuit base plate, and microwave circuit base plate and preparation method thereof
CN111187478A
Preparation method of low-loss ultrathin PTFE microwave dielectric substrate
CN117429141A
Conductive sheet and method for producing the same
JP2013080590A
Electrical conducting, non-woven textile fabric
US20020058179A1
Composite material, high-frequency circuit baseboard made therefrom and production method thereof
WO2012151820A1