Ferroelectric multilayer film with crystalline and non-crystalline homojunctions and preparation method of ferroelectric multilayer film

By doping rare earth elements into the PZT ferroelectric thin film to form a homojunction ferroelectric multilayer film with different crystalline states, the problems of high residual polarization strength and low breakdown electric field strength in PZT materials are solved, and the energy storage density is improved.

CN118899166APending Publication Date: 2024-11-05SOUTHWEAT UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410824428.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The residual polarization strength of PZT ferroelectric film materials is high, resulting in a low breakdown electric field strength, affecting the energy storage density.

Method used

Using a homojunction ferroelectric multilayer film with crystalline and non-crystalline, different crystalline states are formed by doping rare earth elements into the first lead zirconium titanate layer and the second lead zirconium titanate layer to reduce the residual polarization strength. And increase the breakdown electric field strength. The specific method includes a rare earth element doping amount in the first lead zirconium titanate layer, a rare earth element doping amount in the second lead zirconium titanate layer, and a stacked structure is formed by lamination arrangement.

Benefits of technology

The low residual polarization strength and high breakdown electric field strength of the homojunction ferroelectric multilayer film are achieved, thereby improving the energy storage density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899166A_ABST
    Figure CN118899166A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of thin film dielectric energy storage materials, in particular to a crystalline and non-crystalline homojunction ferroelectric multilayer film and a preparation method thereof. The homojunction ferroelectric multilayer film comprises a first lead zirconate titanate layer and a second lead zirconate titanate layer which are arranged in a stacked mode. The first lead zirconate titanate layer and the second lead zirconate titanate layer are doped with rare earth elements respectively, and the doping amount of the rare earth elements in the first lead zirconate titanate layer is smaller than the doping amount of the rare earth elements in the second lead zirconate titanate layer, so that the crystalline states of the first lead zirconate titanate layer and the second lead zirconate titanate layer are different; by using the amorphous first lead zirconate titanate layer and the crystalline second lead zirconate titanate layer, a homojunction ferroelectric multilayer film product with the breakdown strength of 5.2 MV / cm or above and the energy storage density of 50 J / cm < 3 > or above can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of thin film dielectric energy storage materials, and in particular to a ferroelectric multilayer film having a crystalline and amorphous homojunction and a preparation method thereof. Background Art

[0002] Among the energy storage devices such as batteries, fuel cells, electrochemical capacitors and dielectric capacitors, dielectric capacitors show advantages such as high power density, ultra-fast charging speed, ultra-fast discharging speed, long service life, all-solid state, and excellent reliability. Based on the characteristics of dielectric thin film materials that can improve leakage current characteristics and microstructure density, the breakdown strength of dielectric thin film materials can be much higher than that of corresponding ceramic bulk materials, which makes dielectric thin films show higher energy storage density than ceramic bulk materials, but their energy density is still lower than other energy storage devices. Therefore, how to improve the energy storage density of dielectric thin film dielectrics has become an urgent problem that needs to be solved in dielectric thin film dielectrics.

[0003] Among the many dielectric thin film dielectric materials, lead zirconate titanate PbZr 1-x Ti x O 3 (PZT) material is a typical ABO 3 One of the perovskite-type lead-based ferroelectric materials, its energy storage density can be expressed by the formula: Approximate calculations show that the energy storage density depends mainly on the difference between the saturation polarization and the residual polarization and the breakdown strength, among which the storage density is closely related to the breakdown strength. As a ferroelectric thin film material, PZT has a large saturation polarization strength (>60μC / cm 2 ), which makes PZT have certain application potential in the field of energy storage. However, as a typical ferroelectric thin film material, PZT has a large residual polarization strength (about 45μC / cm 2 ) and lower breakdown electric field strength (about 0.6MV / cm), which will result in a lower recoverable energy density of the PZT film, affecting the final energy storage density. In addition, a well-crystallized PZT film has a large polarization strength but a poor breakdown electric field strength. Conversely, a non-crystalline PZT film has a high breakdown electric field strength and a small polarization strength. Therefore, the preparation of a crystalline and non-crystalline multilayer film is a feasible composite path to simultaneously obtain good polarization strength and breakdown electric field strength. Summary of the invention

[0004] The present application provides a crystalline and non-crystalline homojunction ferroelectric multilayer film and a preparation method thereof to solve the following technical problem: how to reduce the residual polarization intensity of PZT ferroelectric thin film material while improving the breakdown strength of PZT.

[0005] In the first aspect, the present application provides a homojunction ferroelectric multilayer film having crystallinity and non-crystallization, wherein the homojunction ferroelectric multilayer film comprises a first lead zirconate titanate layer and a second lead zirconate titanate layer which are stacked; the first lead zirconate titanate layer and the second lead zirconate titanate layer are doped with rare earth elements, respectively, and the doping amount of the rare earth elements in the first lead zirconate titanate layer is less than the doping amount of the rare earth elements in the second lead zirconate titanate layer, so that the crystallinity of the first lead zirconate titanate layer and the second lead zirconate titanate layer are different.

[0006] Optionally, the doping amount of the rare earth element in the first lead zirconate titanate layer is ≤5%, and the doping amount of the rare earth element in the second lead zirconate titanate layer is ≥10%.

[0007] Optionally, the rare earth element includes cerium.

[0008] Optionally, the thickness of the first lead zirconate titanate layer and the second lead zirconate titanate layer are 38 nm to 54 nm respectively.

[0009] Optionally, the number of layers of the homojunction ferroelectric multilayer film is 5, and the innermost layer and the outermost layer of the homojunction ferroelectric multilayer film are the first lead zirconate titanate layer or the second lead zirconate titanate layer.

[0010] Optionally, the thickness of the homojunction ferroelectric multilayer film is 190 nm to 270 nm.

[0011] In a second aspect, the present application provides a method for preparing the homojunction ferroelectric multilayer film according to the first aspect, the method comprising:

[0012] Mixing rare earth element salts and lead sources with different contents to prepare a first precursor solution or a second precursor solution containing rare earth elements;

[0013] The first precursor solution containing a rare earth element and the second precursor solution containing a rare earth element are mixed with acetylacetone respectively, and then a zirconium source and a titanium source are added and mixed respectively to obtain a first mixed solution and a second mixed solution;

[0014] The first mixed solution and the second mixed solution are respectively fixed to volume, and then filtered and aged to obtain a first composite material precursor solution and a second composite material precursor;

[0015] The first composite material precursor solution and the second composite material precursor are respectively subjected to spin coating, and then dried, pyrolyzed and annealed to obtain a first lead zirconate titanate layer and a second lead zirconate titanate layer;

[0016] The first lead zirconate titanate layer and the second lead zirconate titanate layer are stacked to obtain a homojunction ferroelectric multilayer film.

[0017] Optionally, the molar ratio of the rare earth element salt to the lead source is 1:9 to 1:19.

[0018] Optionally, the rotation speed of the spin coating is 3900 r / min to 4200 r / min, and the time of the spin coating is 28 s to 32 s.

[0019] Optionally, the annealing temperature is 550° C. to 600° C., and the annealing time is 10 min to 30 min.

[0020] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0021] An embodiment of the present application provides a homojunction ferroelectric multilayer film having both crystalline and non-crystalline properties. By controlling the difference in rare earth element doping amounts in the first lead zirconate titanate layer and the second lead zirconate titanate layer, the first lead zirconate titanate layer and the second lead zirconate titanate layer can be in different crystalline states (crystalline and non-crystalline), and the first lead zirconate titanate layer and the second lead zirconate titanate layer in different crystalline states can provide different material properties. For example, the crystalline lead zirconate titanate has a better saturation polarization intensity, which can reduce the residual polarization intensity of the lead zirconate titanate, while the non-crystalline lead zirconate titanate has a good breakdown electric field strength. In addition, the stacked arrangement can combine the different properties of the first lead zirconate titanate layer and the second lead zirconate titanate layer to enable the homojunction ferroelectric multilayer film formed by the two to have a lower residual polarization intensity and a higher breakdown electric field strength, thereby improving the energy storage density of the final homojunction ferroelectric multilayer film. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0023] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0024] Figure 1 A schematic diagram of a product having a crystalline and amorphous homojunction ferroelectric multilayer film provided in an embodiment of the present application;

[0025] Figure 2 A schematic flow chart of a method for preparing a homojunction ferroelectric multilayer film provided in an embodiment of the present application;

[0026] Figure 3 A graph showing the test results of the hysteresis loop of the single crystalline homojunction ferroelectric multilayer film provided in Comparative Examples 1 and 2 of the present application;

[0027] Figure 4 This is a graph showing the test results of a hysteresis loop of a homojunction ferroelectric multilayer film having crystallization and non-crystallization provided in Example 1 of the present application. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0029] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be understood as a rigid limitation on the scope of the present application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within the range; for example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which applies regardless of the range; in addition, whenever a numerical range is indicated in this document, it is meant to include any cited numbers (fractions or integers) within the indicated range.

[0030] In this document, the terms "including" and "comprising" mean "including but not limited to". Relational terms such as "first" and "second" are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations. Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0031] Figure 1 A schematic diagram of a product having a crystalline and amorphous homojunction ferroelectric multilayer film provided in an embodiment of the present application is exemplarily shown;

[0032] like Figure 1As shown, an embodiment of the present application provides a homojunction ferroelectric multilayer film having crystallinity and non-crystallization, wherein the homojunction ferroelectric multilayer film includes a first lead zirconate titanate layer and a second lead zirconate titanate layer stacked in layers; the first lead zirconate titanate layer and the second lead zirconate titanate layer are doped with rare earth elements, respectively, and the doping amount of the rare earth elements in the first lead zirconate titanate layer is less than the doping amount of the rare earth elements in the second lead zirconate titanate layer, so that the first lead zirconate titanate layer and the second lead zirconate titanate layer have different crystal states.

[0033] In some optional embodiments, the doping amount of the rare earth element in the first lead zirconate titanate layer is ≤5%, and the doping amount of the rare earth element in the second lead zirconate titanate layer is ≥10%;

[0034] In these embodiments, the doping amount of rare earth elements in the first lead zirconate titanate layer can be ≤5%, which can cause the crystalline state of the first lead zirconate titanate layer to be in an amorphous state, and the first lead zirconate titanate layer in the amorphous state has a good breakdown electric field strength. In addition, the doping amount of rare earth elements in the second lead zirconate titanate layer can be ≥10%, which can cause the crystalline state of the second lead zirconate titanate layer to be in a crystalline state, and the second lead zirconate titanate layer in the crystalline state has a good saturation polarization strength, so that the stacked first lead zirconate titanate layer and the second lead zirconate titanate layer can be used to achieve low residual polarization strength and high breakdown electric field strength of the homojunction ferroelectric multilayer film, thereby improving the energy storage density of the final homojunction ferroelectric multilayer film.

[0035] In some optional embodiments, the rare earth element includes cerium;

[0036] In these optional embodiments, the rare earth element may include cerium, and different doping amounts of cerium can be used to adjust the crystallinity of the first lead zirconate titanate layer and the second lead zirconate titanate layer to ultimately obtain an amorphous first lead zirconate titanate layer and a crystalline second lead zirconate titanate layer. In addition, the addition of rare earth elements can also increase the energy storage density of each lead zirconate titanate layer to ultimately increase the energy storage density of the homojunction ferroelectric multilayer film.

[0037] In some optional embodiments, the thickness of the first lead zirconate titanate layer and the second lead zirconate titanate layer are 38 nm to 54 nm respectively;

[0038] In these embodiments, the thickness of the first lead zirconate titanate layer and the second lead zirconate titanate layer can be 38nm to 54nm, respectively, which can ensure that the first lead zirconate titanate layer and the second lead zirconate titanate layer have sufficient thickness. The first lead zirconate titanate layer with sufficient thickness can effectively improve the breakdown strength of the homojunction ferroelectric multilayer film to reduce the residual polarization intensity of the homojunction ferroelectric multilayer film. In addition, the second lead zirconate titanate layer with sufficient thickness can effectively improve the saturation polarization intensity of the homojunction ferroelectric multilayer film.

[0039] The thickness of the first lead zirconate titanate layer and the second lead zirconate titanate layer can be 38nm, 39nm, 40nm, 41nm, 42nm, 43nm, 44nm, 45nm, 46nm, 47nm, 48nm, 49nm, 50nm, 51nm, 52nm, 53nm, 54nm or 55nm respectively.

[0040] In some optional embodiments, the number of layers of the homojunction ferroelectric multilayer film is 5, and the innermost layer and the outermost layer of the homojunction ferroelectric multilayer film are the first lead zirconate titanate layer or the second lead zirconate titanate layer;

[0041] In these embodiments, the number of layers of the homojunction ferroelectric multilayer film can be 5 layers, and the innermost layer and the outermost layer of the homojunction ferroelectric multilayer film can be the first lead zirconate titanate layer or the second lead zirconate titanate layer, and a homojunction ferroelectric multilayer film structure of the second lead zirconate titanate layer + the first lead zirconate titanate layer + the second lead zirconate titanate layer + the first lead zirconate titanate layer + the second lead zirconate titanate layer can be formed, or a homojunction ferroelectric multilayer film structure of the first lead zirconate titanate layer + the second lead zirconate titanate layer + the first lead zirconate titanate layer + the second lead zirconate titanate layer + the first lead zirconate titanate layer, so as to enable the homojunction ferroelectric multilayer film to have sufficient thickness and a uniformly distributed structure, thereby improving the energy storage density of the homojunction ferroelectric multilayer film.

[0042] In some optional embodiments, the thickness of the homojunction ferroelectric multilayer film is 190 nm to 270 nm;

[0043] In these embodiments, the thickness of the homojunction ferroelectric multilayer film can be 190nm to 270nm, which can enable the homojunction ferroelectric multilayer film to have enough first lead zirconate titanate layers and second lead zirconate titanate layers, thereby improving the energy storage density of the homojunction ferroelectric multilayer film.

[0044] The thickness of the homojunction ferroelectric multilayer film may be 190 nm, 200 nm, 210 nm, 220 nm, 230 nm, 240 nm, 250 nm, 260 nm or 270 nm.

[0045] Figure 2 A schematic flow chart of a method for preparing a homojunction ferroelectric multilayer film provided in an embodiment of the present application is exemplarily shown;

[0046] like Figure 2 As shown, the present application provides a method for preparing the homojunction ferroelectric multilayer film, the method comprising:

[0047] S1. Mixing different contents of rare earth element salts and lead sources to prepare a first precursor solution or a second precursor solution containing a rare earth element;

[0048] S2. The first precursor solution containing a rare earth element and the second precursor solution containing a rare earth element are mixed with acetylacetone, and then a zirconium source and a titanium source are added and mixed to obtain a first mixed solution and a second mixed solution;

[0049] S3. respectively adjusting the volume of the first mixed solution and the second mixed solution, and then filtering and aging them respectively to obtain a first composite material precursor solution and a second composite material precursor;

[0050] S4. Spin coating the first composite material precursor solution and the second composite material precursor, respectively, and then drying, pyrolyzing and annealing them, respectively, to obtain a first lead zirconate titanate layer and a second lead zirconate titanate layer;

[0051] S5. The first lead zirconate titanate layer and the second lead zirconate titanate layer are stacked to obtain a homojunction ferroelectric multilayer film.

[0052] This method is a method for preparing the above-mentioned homojunction ferroelectric multilayer film. The specific structure of the homojunction ferroelectric multilayer film can refer to the above-mentioned embodiment. Since the homojunction ferroelectric multilayer film adopts part or all of the technical solutions of the above-mentioned embodiments, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be repeated here one by one.

[0053] It should be noted that the first precursor solution or the second precursor solution, the first mixed solution and the second mixed solution, and the first composite material precursor solution and the second composite material precursor differ only in the content of the rare earth element.

[0054] It should be noted that the mass ratio of the zirconium source to the titanium source can be 0.52:0.48.

[0055] It should be noted that the mixing time can be 3.5 hours.

[0056] It should be noted that a disposable syringe filter may be used for the filtration, and the pore size of the filter may be 0.22 μm.

[0057] It should be noted that the aging time can be 24 hours.

[0058] It should be noted that the heating equipment for the spin coating can be a heating magnetic stirrer, a desktop glue baking machine and a tubular resistance furnace; the drying temperature can be 200°C, and the drying time can be 5 minutes; the pyrolysis temperature can be 450°C, and the pyrolysis time can be 10 minutes.

[0059] It should be noted that if tiny impurities appear during the spin coating process, it is necessary to use a rubber-tipped dropper to suck out the impurities, which causes a certain difference in thickness between the first lead zirconate titanate layer and the second lead zirconate titanate layer.

[0060] In some optional embodiments, the molar ratio of the rare earth element salt to the lead source is 1:9 to 1:19;

[0061] In these embodiments, the molar ratio of the rare earth element salt to the lead source can be 1:9 to 1:19, which can cause the lead source to be excessive so as to cause sufficient rare earth elements to be present in the final first lead zirconate titanate layer and the second lead zirconate titanate layer, thereby causing the rare earth element doping amount of the first lead zirconate titanate layer to be ≤5% and the rare earth element doping amount of the second lead zirconate titanate layer to be ≥10%, so as to finally obtain an amorphous first lead zirconate titanate layer and a crystalline second lead zirconate titanate layer.

[0062] The molar ratio of the rare earth element salt to the lead source can be 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18 or 1:19.

[0063] In some optional embodiments, the rotation speed of the spin coating is 3900r / min to 4200r / min, and the time of the spin coating is 28s to 32s;

[0064] In these embodiments, the spin coating rotation speed can be 3900r / min~4200r / min, and the spin coating time can be 28s~32s. The first lead zirconate titanate layer and the second lead zirconate titanate layer can be evenly distributed by spin coating to promote the rare earth elements to be evenly distributed in the first lead zirconate titanate layer and the second lead zirconate titanate layer.

[0065] The rotation speed of the spin coating can be 3900r / min, 3950r / min, 4000r / min, 4050r / min, 4100r / min, 4150r / min or 4200r / min.

[0066] The spin coating time can be 28s, 29s, 30s, 31s or 32s.

[0067] In some optional embodiments, the annealing temperature is 550° C. to 600° C., and the annealing time is 10 min to 30 min;

[0068] In these embodiments, the annealing temperature can be 550°C to 600°C, and the annealing time can be 10 minutes to 30 minutes. Annealing can be used to enable the first lead zirconate titanate layer and the second lead zirconate titanate layer to be fully formed, so as to ultimately obtain an amorphous first lead zirconate titanate layer and a crystalline second lead zirconate titanate layer, thereby ultimately improving the energy storage density of the homojunction ferroelectric multilayer film.

[0069] The annealing temperature may be 550°C, 560°C, 570°C, 580°C, 590°C or 600°C.

[0070] The annealing time can be 10 min, 15 min, 20 min, 25 min or 30 min.

[0071] The present application is further described below in conjunction with specific examples. The experimental methods in the following examples that do not specify specific conditions are usually measured according to industry standards; if there are no corresponding industry standards, they are carried out according to common international standards, conventional conditions, or conditions recommended by the manufacturer.

[0072] Example 1

[0073] like Figure 1 As shown, a homojunction ferroelectric multilayer film having crystallization and non-crystallization, the homojunction ferroelectric multilayer film comprising a second lead zirconate titanate layer + a first lead zirconate titanate layer + a second lead zirconate titanate layer + a first lead zirconate titanate layer + a second lead zirconate titanate layer stacked; the first lead zirconate titanate layer and the second lead zirconate titanate layer are doped with a rare earth element cerium, respectively, and the doping amount of the rare earth element in the first lead zirconate titanate layer is 5% (denoted as PC 0.05 ZT, referred to as "5"), the doping amount of rare earth elements in the second lead zirconate titanate layer is 10%, denoted as PC 0.1 ZT, referred to as "1" for short), so that the first lead zirconate titanate layer is amorphous and the second lead zirconate titanate layer is crystalline.

[0074] The thickness of the homojunction ferroelectric multilayer film is 250 nm.

[0075] like Figure 2 As shown, a method for preparing a homojunction ferroelectric multilayer film comprises:

[0076] S1. Mixing rare earth element salts and lead sources with different contents to prepare a first precursor solution or a second precursor solution containing rare earth elements; the specific steps include: 1) Weighing 6.1453 g of lead acetate and 0.4759 g of cerium acetate, respectively, and then adding the lead acetate and cerium acetate to 18 mL of propionic acid solution, heating and stirring at 90°C with a magnetic stirrer for 50 min until the solid phase is dissolved, to obtain a second precursor solution of a clear, colorless and transparent solution, and then cooling to room temperature and stirring for use; 2) Weighing 6.4867 g of lead acetate and 0.2379 g of cerium acetate, respectively, and then adding the lead acetate and cerium acetate to 18 mL of propionic acid solution, heating and stirring at 90°C with a magnetic stirrer for 50 min until the solid phase is dissolved, to obtain a first precursor solution of a clear, colorless and transparent solution, and then cooling to room temperature and stirring for use;

[0077] S2. The first precursor solution containing a rare earth element and the second precursor solution containing a rare earth element were mixed with 1 mL of acetylacetone, and then a zirconium source and a titanium source were added and mixed to obtain a first mixed solution and a second mixed solution;

[0078] S3. The first mixed solution and the second mixed solution are respectively fixed to volume, and then filtered at 0.22 μm and aged for 24 h to obtain a first composite material precursor solution and a second composite material precursor;

[0079] S4. Spin coating the first composite material precursor solution and the second composite material precursor, respectively, and then drying on a 200° C. hot plate for 5 min and pyrolyzing in a 450° C. glue baking machine for 10 min to obtain a first lead zirconate titanate layer and a second lead zirconate titanate layer, respectively;

[0080] S5. The first lead zirconate titanate layer and the second lead zirconate titanate layer are stacked by spin coating layer by layer to obtain a homojunction ferroelectric multilayer film.

[0081] The rotation speed of the spin coating is 4000r / min, and the time of the spin coating is 30s.

[0082] The annealing temperature is 600°C and the annealing time is 10 min.

[0083] Example 2

[0084] Based on the contents disclosed in Example 1, the following operations are further performed:

[0085] The annealing temperature is 600°C and the annealing time is 30 minutes.

[0086] Example 3

[0087] Based on the contents disclosed in Example 1, the following operations are further performed:

[0088] The annealing temperature is 550°C and the annealing time is 10 min.

[0089] Example 4

[0090] Based on the contents disclosed in Example 1, the following operations are further performed:

[0091] The annealing temperature is 550°C and the annealing time is 30 min.

[0092] Example 5

[0093] Based on the contents disclosed in Example 1, the following operations are further performed:

[0094] The rotation speed of the spin coating is 3900r / min, and the time of the spin coating is 32s.

[0095] Example 6

[0096] Based on the contents disclosed in Example 1, the following operations are further performed:

[0097] The rotation speed of the spin coating is 4200r / min, and the time of the spin coating is 28s.

[0098] Comparative Example 1

[0099] Based on the contents disclosed in Example 1, the following operations are further performed:

[0100] A 5-layer homojunction ferroelectric multilayer film is formed using only the first lead zirconate titanate layer.

[0101] Comparative Example 2

[0102] Based on the contents disclosed in Example 1, the following operations are further performed:

[0103] A 5-layer homojunction ferroelectric multilayer film was formed using only the second lead zirconate titanate layer.

[0104] Comparative Example 3

[0105] Based on the contents disclosed in Example 1, the following operations are further performed:

[0106] The homojunction ferroelectric multilayer film comprises a first lead zirconate titanate layer+a second lead zirconate titanate layer+a first lead zirconate titanate layer+a second lead zirconate titanate layer+a first lead zirconate titanate layer which are stacked.

[0107] Comparative Example 4

[0108] Based on the contents disclosed in Example 1, the following operations are further performed:

[0109] The annealing temperature is 500°C and the annealing time is 50 min.

[0110] Comparative Example 5

[0111] Based on the contents disclosed in Example 1, the following operations are further performed:

[0112] The annealing temperature is 650°C and the annealing time is 5 min.

[0113] Related experiments and effect data:

[0114] The breakdown strength and energy storage density of the homojunction ferroelectric multilayer films obtained in various embodiments and comparative examples were statistically analyzed, and the results are shown in Table 1.

[0115] Table 1 Breakdown strength and energy storage density of homojunction ferroelectric multilayer films obtained in various embodiments and comparative examples

[0116]

[0117] As shown in Table 1, the amorphous first lead zirconate titanate layer and the crystalline second lead zirconate titanate layer can be obtained at the annealing temperature of each embodiment. In addition, the first lead zirconate titanate layer and the second lead zirconate titanate layer are stacked in an interlaced manner, which can improve the breakdown strength of the homojunction ferroelectric multilayer film by ≥5.2MV / cm, and improve the energy storage density of the homojunction ferroelectric multilayer film by ≥50J / cm 3 .

[0118] Figure 3 The hysteresis loop test result diagram of the single crystalline homojunction ferroelectric multilayer film provided in Comparative Examples 1 and 2 of the present application is exemplarily shown;

[0119] Figure 4 The hysteresis loop test result diagram of a crystalline and non-crystalline homojunction ferroelectric multilayer film provided in Example 1 of the present application is exemplarily shown;

[0120] In addition, the homogeneous ferroelectric multilayer films obtained in Example 1, Comparative Example 1 and Comparative Example 2 were subjected to hysteresis loop tests. The results are as follows: Figure 3 and Figure 4 As shown, this illustrates that the homojunction ferroelectric multilayer film provided in the embodiment of the present application also has a relatively high saturation polarization intensity.

[0121] In summary, the embodiment of the present application provides a ferroelectric multilayer film having a crystalline and amorphous homojunction, which uses an amorphous first lead zirconate titanate layer and a crystalline second lead zirconate titanate layer, and can obtain a breakdown strength of more than 5.2 MV / cm and an energy storage density of 50 J / cm. 3 The above homojunction ferroelectric multilayer film products.

[0122] In addition, the method for preparing a homojunction ferroelectric multilayer film provided in the embodiment of the present application has the advantages of a simple preparation process and convenient operation.

[0123] The above is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. It will be apparent to those skilled in the art that various modifications to these embodiments are possible, and the general principles defined in the present application can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to these embodiments shown in the present application, but will conform to the widest scope consistent with the principles and novel features applied for by the present application.

Claims

1. A ferroelectric homojunction multilayer film having crystalline and amorphous components, characterized in that: The homojunction ferroelectric multilayer film includes a first lead zirconate titanate layer and a second lead zirconate titanate layer which are stacked; the first lead zirconate titanate layer and the second lead zirconate titanate layer are doped with rare earth elements respectively, and the doping amount of the rare earth elements in the first lead zirconate titanate layer is less than the doping amount of the rare earth elements in the second lead zirconate titanate layer, so that the crystal states of the first lead zirconate titanate layer and the second lead zirconate titanate layer are different.

2. The homojunction ferroelectric multilayer film according to claim 1, characterized in that: The doping amount of the rare earth element in the first lead zirconate titanate layer is ≤5%, and the doping amount of the rare earth element in the second lead zirconate titanate layer is ≥10%.

3. The homojunction ferroelectric multilayer film according to claim 1 or 2, characterized in that: The rare earth element includes cerium.

4. The homojunction ferroelectric multilayer film according to claim 1, characterized in that: The thickness of the first lead zirconate titanate layer and the second lead zirconate titanate layer are 38 nm to 54 nm respectively.

5. The homojunction ferroelectric multilayer film according to claim 1, characterized in that: The number of layers of the homojunction ferroelectric multilayer film is 5, and the innermost layer and the outermost layer of the homojunction ferroelectric multilayer film are the first lead zirconate titanate layer or the second lead zirconate titanate layer.

6. The homojunction ferroelectric multilayer film according to claim 5, characterized in that: The thickness of the homojunction ferroelectric multilayer film is 190nm-270nm.

7. A method for preparing the homojunction ferroelectric multilayer film according to any one of claims 1 to 6, characterized in that: The method comprises: Mixing rare earth element salts and lead sources with different contents to prepare a first precursor solution or a second precursor solution containing rare earth elements; The first precursor solution containing a rare earth element and the second precursor solution containing a rare earth element are mixed with acetylacetone respectively, and then a zirconium source and a titanium source are added and mixed respectively to obtain a first mixed solution and a second mixed solution; The first mixed solution and the second mixed solution are respectively fixed to volume, and then filtered and aged to obtain a first composite material precursor solution and a second composite material precursor; The first composite material precursor solution and the second composite material precursor are respectively subjected to spin coating, and then dried, pyrolyzed and annealed to obtain a first lead zirconate titanate layer and a second lead zirconate titanate layer; The first lead zirconate titanate layer and the second lead zirconate titanate layer are stacked to obtain a homojunction ferroelectric multilayer film.

8. The method according to claim 7, characterized in that The molar ratio of the rare earth element salt to the lead source is 1:9 to 1:

19.

9. The method according to claim 7, characterized in that: The rotation speed of the spin coating and the glue spinning is 3900r / min-4200r / min, and the time of the spin coating and the glue spinning is 28s-32s.

10. The method according to claim 7, characterized in that The annealing temperature is 550° C. to 600° C., and the annealing time is 10 min to 30 min.