Single-layer chip ceramic dielectric capacitor and preparation method and application thereof
By using the structure of the front Au layer and the back Pt layer in a single-layer chip porcelain dielectric capacitor, the problems of high material costs and preparation complexity in traditional structures are solved, and the effect of reducing costs and maintaining electrical performance is achieved.
Patent Information
- Application Number
- CN202411266169.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-05
AI Technical Summary
The existing single-layer chip porcelain dielectric capacitors have high material costs during welding, and the traditional TiW+Ni+Au film layer structure causes the thickness of the back Au layer to exceed 3μm, which increases the production complexity and cost.
Using the structure of the front Au layer and the back Pt layer, the TiW layer, NiV layer (or NiV alloy), Au layer and Pt layer are sputtered on the ceramic substrate in turn to control the thickness of the Au layer ≤2000nm and the thickness of the Pt layer ≤600nm to reduce the thickness of the Material cost.
The material cost is reduced, while maintaining the same electrical properties and solderability as the traditional TiW+Ni+Au film layer structure, simplifying the preparation process, and reducing the needs of subsequent granular picking and lithography processes.
Smart Images

Figure CN118899167A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of capacitors, and in particular to a single-layer chip ceramic capacitor and a preparation method and application thereof. Background Art
[0002] Single-layer chip ceramic capacitors are widely used in peripheral circuits of GaN or GaAs chips, wireless communications, optical fiber communications and other micro-assembly circuits, providing thin-film integrated packaging products for semiconductor integrated circuits, 5G communications, aerospace and other fields. In order to ensure that the device packaging process can meet the welding methods such as gold wire bonding and eutectic welding, and at the same time have excellent electrical properties and reliability, most single-layer chip ceramic capacitors on the market currently use gold (Au) electrodes on both sides, and the front and back sides usually use TiW+Ni+Au film layer structures, and the Au layer thickness is generally required to be >3μm, which has a high material cost. Summary of the invention
[0003] The purpose of the present invention is to provide a single-layer chip ceramic capacitor and its preparation method and application. In the present invention, the front and back sides of the single-layer chip ceramic capacitor adopt different film layer structures, only the front side is provided with an Au layer, and its thickness is ≤2000nm, and the thickness of the Pt layer on the back side is ≤600nm, which effectively reduces the material cost.
[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0005] The present invention provides a single-layer chip ceramic capacitor, comprising an Au layer, a barrier layer, a first TiW layer, a ceramic substrate, a second TiW layer and a Pt layer stacked in sequence, wherein the barrier layer comprises a NiV layer, the thickness of the Au layer is ≤2000nm, and the thickness of the Pt layer is ≤600nm.
[0006] Preferably, the barrier layer further includes an Al layer or a Cu layer stacked with the NiV layer. When the barrier layer includes the Al layer or the Cu layer, the NiV layer is in contact with the Au layer.
[0007] Preferably, the barrier layer has a thickness of 500-1500 nm; and the Al layer and the Cu layer have thicknesses of 200-600 nm independently.
[0008] Preferably, the NiV layer is formed of a NiV alloy, and the mass fraction of Ni in the NiV alloy is 90-95%.
[0009] Preferably, the first TiW layer and the second TiW layer are formed of a TiW alloy, and the mass fraction of Ti in the TiW alloy forming the first TiW layer and the second TiW layer is independently 80-95%.
[0010] Preferably, the thickness of the first TiW layer and the second TiW layer are independently 50-200 nm.
[0011] Preferably, the thickness of the Au layer is 1300-2000 nm, and the thickness of the Pt layer is 300-600 nm.
[0012] The present invention provides a method for preparing the single-layer chip ceramic capacitor described in the above technical solution, comprising the following steps:
[0013] sputtering a first TiW layer, a barrier layer, and an Au layer in sequence on one surface of a ceramic substrate, and sputtering a second TiW layer and a Pt layer in sequence on the other surface of the ceramic substrate to obtain a metallized ceramic substrate;
[0014] The metallized ceramic substrate is subjected to a dicing process to obtain the single-layer chip ceramic capacitor.
[0015] Preferably, the sputtering method of the first TiW layer, the barrier layer, the Au layer, the second TiW layer and the Pt layer is a scanning sputtering method;
[0016] The sputtering power of the first TiW layer is 800-1200W, and the number of scans is 20-30 times;
[0017] The sputtering power of the Au layer is 300-600W, and the number of scans is 180-220 times;
[0018] The sputtering power of the second TiW layer is 800-1200W, and the number of scans is 20-30 times;
[0019] The sputtering power of the Pt layer is 600-1000W, and the number of scans is 80-100 times;
[0020] When the barrier layer is a NiV layer, the sputtering power of the barrier layer is 800 to 1200 W, and the number of scans is 45 to 55 times;
[0021] When the barrier layer is a stacked NiV layer and an Al layer, or a stacked NiV layer and a Cu layer, the sputtering power of the NiV layer is 800-1200W, and the scanning number is 25-35 times; the sputtering power of the Al layer is 1500-2000W, and the scanning number is 30-40 times; the sputtering power of the Cu layer is 1000-1600W, and the scanning number is 30-40 times.
[0022] The present invention provides the application of the single-layer chip ceramic capacitor described in the above technical scheme or the single-layer chip ceramic capacitor prepared by the preparation method described in the above technical scheme in semiconductor integrated circuits, 5G communications or aerospace fields.
[0023] The present invention provides a single-layer chip ceramic capacitor, comprising an Au layer, a barrier layer, a first TiW layer, a ceramic substrate, a second TiW layer and a Pt layer stacked in sequence, wherein the barrier layer comprises a NiV layer, the thickness of the Au layer is ≤2000nm, and the thickness of the Pt layer is ≤600nm. In the present invention, the front and back sides of the single-layer chip ceramic capacitor adopt different film layer structures, only the front side is provided with an Au layer, and its thickness is ≤2000nm, and the thickness of the Pt layer on the back side is ≤600nm, which effectively reduces the material cost; and the electrical performance indicators, weldability, and reliability verification of the single-layer chip ceramic capacitor provided by the present invention are consistent with those of traditional front and back TiW+Ni+Au film layer structure products, which is convenient for large-scale promotion and use. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Schematic diagram of the structure of a single-layer chip ceramic capacitor in the present invention, in which 1 is an Au layer, 2 is a barrier layer, 3 is a first TiW layer, 4 is a ceramic substrate, 5 is a second TiW layer, and 6 is a Pt layer;
[0025] Figure 2 This is a flow chart of preparing a single-layer chip ceramic capacitor in Example 1 of the present invention. DETAILED DESCRIPTION
[0026] The present invention provides a single-layer chip ceramic capacitor, comprising an Au layer, a barrier layer, a first TiW layer, a ceramic substrate, a second TiW layer and a Pt layer stacked in sequence, wherein the barrier layer comprises a NiV layer, the thickness of the Au layer is ≤2000nm, and the thickness of the Pt layer is ≤600nm.
[0027] The single-layer chip ceramic capacitor provided by the present invention includes a ceramic substrate, on one surface (front side, or A side) of which a first TiW layer, a barrier layer and an Au layer are sequentially stacked, and on the other surface (back side, or B side) of which a second TiW layer and a Pt layer are sequentially stacked, wherein the first TiW layer and the second TiW layer serve as adhesion layers, and the Au layer and the Pt layer serve as electrodes. Each layer is described in detail below.
[0028] In the present invention, the first TiW layer is formed of a TiW alloy, and the mass fraction of Ti in the TiW alloy is preferably 80-95%, more preferably 85-95%, and further preferably 90-95% (when the mass fraction of Ti in the TiW alloy is 95%, the mass ratio of Ti to W in the first TiW layer is 95:5). In the present invention, the thickness of the first TiW layer is preferably 50-200 nm, more preferably 100-150 nm. The present invention preferably controls the element composition in the TiW alloy within the above range, and controls the thickness of the first TiW layer within the above range, which is conducive to ensuring that the first TiW layer has a better bonding effect as an adhesion layer and improves the bonding strength.
[0029] In the present invention, the barrier layer includes a NiV layer, and the barrier layer preferably also includes an Al layer or a Cu layer stacked with the NiV layer. When the barrier layer includes an Al layer or a Cu layer, the NiV layer is in contact with the Au layer, that is, the barrier layer can be a NiV layer, or a NiV layer + an Al layer, or a NiV layer + a Cu layer. In the present invention, the NiV layer is formed by a NiV alloy, and the mass fraction of Ni in the NiV alloy is preferably 90 to 95%, more preferably 92 to 94%, and further preferably 93% (at this time, the mass ratio of Ni to V in the NiV layer is 93:7). In the present invention, the thickness of the barrier layer is preferably 500 to 1500 nm, more preferably 750 to 1300 nm, and further preferably 850 to 1100 nm; the thickness of the Al layer and the Cu layer are independently preferably 200 to 600 nm, more preferably 350 to 600 nm, and further preferably 450 to 600 nm. In the present invention, when the barrier layer is a NiV layer, the thickness of the barrier layer is the thickness of the NiV layer. When the barrier layer is a NiV layer + an Al layer, or a NiV layer + a Cu layer, the thickness of the barrier layer is the total thickness of the NiV layer + the Al layer, or the total thickness of the NiV layer + the Cu layer. In the present invention, the barrier layer uses a NiV alloy to replace the Ni layer in the traditional single-layer chip ceramic capacitor, and appropriately increases the thickness of the barrier layer, which can replace the role of a part of the Au layer, thereby reducing the thickness of the Au layer to within 2000nm, which is beneficial to reducing material costs; at the same time, the barrier layer in the present invention can also use a cheaper Cu or Al and NiV alloy combination, which is beneficial to further reduce material costs.
[0030] In the present invention, the thickness of the Au layer is ≤2000 nm, preferably 1300 to 2000 nm, more preferably 1300 to 1700 nm, and further preferably 1300 to 1500 nm.
[0031] In the present invention, the second TiW layer is formed of a TiW alloy, and the mass fraction of Ti in the TiW alloy is preferably 80-95%, more preferably 85-95%, and further preferably 90-95% (when the mass fraction of Ti in the TiW alloy is 95%, the mass ratio of Ti to W in the second TiW layer is 95:5). In the present invention, the thickness of the second TiW layer is preferably 50-200nm, more preferably 100-150nm. The present invention preferably controls the element composition in the TiW alloy within the above range, and controls the thickness of the second TiW layer within the above range, which is conducive to ensuring that the second TiW layer has a better bonding effect as an adhesion layer and improves the bonding force.
[0032] In the present invention, the thickness of the Pt layer is ≤600nm, preferably 300-600nm, more preferably 300-500nm, and further preferably 300-400nm. In the present invention, the outer electrode on the back of the single-layer chip ceramic capacitor is Pt, which is much cheaper than Au, and the thickness of the Pt layer is ≤600nm. The back of the product is used for bonding, which is conducive to further reducing material costs while ensuring that Au can achieve high conductivity and high reliability.
[0033] The present invention provides a method for preparing the single-layer chip ceramic capacitor described in the above technical solution, comprising the following steps:
[0034] sputtering a first TiW layer, a barrier layer, and an Au layer in sequence on one surface of a ceramic substrate, and sputtering a second TiW layer and a Pt layer in sequence on the other surface of the ceramic substrate to obtain a metallized ceramic substrate;
[0035] The metallized ceramic substrate is subjected to a dicing process to obtain the single-layer chip ceramic capacitor.
[0036] The present invention preferably pre-treats the ceramic substrate, and sputters each layer structure on the surface of the pre-treated ceramic substrate to obtain the metallized ceramic substrate. In the present invention, the thickness of the ceramic substrate is preferably 90 to 1500 μm, more preferably 100 to 500 μm, and further preferably 150 to 300 μm. In the present invention, the pre-treatment preferably includes cleaning and baking in sequence. The cleaning of the present invention preferably includes room temperature cleaning and high temperature cleaning in sequence. In the present invention, the number of room temperature cleaning is preferably 3 to 6 times, and each room temperature cleaning preferably includes alkaline cleaning solution cleaning and water cleaning in sequence. The main component of the alkaline cleaning solution used for the alkaline cleaning solution is preferably potassium hydroxide, and the water used for the water cleaning is preferably deionized water; the conditions for each alkaline cleaning solution cleaning independently preferably include: the ultrasonic current is 1.5 to 2.0A, and the cleaning time is 10 to 20min; the time for each water cleaning is independently preferably 4 to 6min. In the present invention, the high-temperature cleaning is preferably high-temperature water cleaning, the water used for the high-temperature water cleaning is preferably deionized water, and the conditions for the high-temperature water cleaning preferably include: water temperature of 65-75°C, ultrasonic current of 1.5-2.0A, and cleaning time of 10-20min. After the cleaning is completed, the present invention preferably uses nitrogen to blow dry the cleaned ceramic substrate, and the baking is performed after the cleanliness inspection is qualified. In the present invention, the baking temperature is preferably 500-1000°C, more preferably 700-800°C; the insulation time is preferably 50-70min, more preferably 55-60min; the heating time from room temperature to the baking temperature is preferably 160-200min, more preferably 170-180min; after the baking is completed, the furnace is cooled to room temperature, and the pretreated ceramic substrate is taken out for subsequent sputtering process. The present invention can fully remove the moisture in the pores of the ceramic substrate by baking, and can also decompose the organic impurities contained therein.
[0037] The present invention sequentially sputters a first TiW layer, a barrier layer and an Au layer on one surface of a ceramic substrate, and sequentially sputters a second TiW layer and a Pt layer on the other surface of the ceramic substrate to obtain a metallized ceramic substrate. The present invention preferably places the ceramic substrate on a sputtering machine tray, puts it into a process chamber and evacuates it, and waits until the vacuum degree in the process chamber is lower than 7.0×10 -7Torr starts sputtering. In the present invention, the sputtering method of the first TiW layer, the barrier layer, the Au layer, the second TiW layer and the Pt layer is preferably a scanning sputtering method; during the sputtering process of the first TiW layer, the barrier layer, the Au layer, the second TiW layer and the Pt layer, the process gas pressure is preferably independently 3 to 9 mTorr, and more preferably 5 to 7 mTorr. In the present invention, the sputtering power of the first TiW layer is preferably 800 to 1200 W, and more preferably 900 to 1000 W; the number of scans is preferably 20 to 30 times, and more preferably 23 to 26 times. In the present invention, when the barrier layer is a NiV layer, the sputtering power of the barrier layer is preferably 800 to 1200 W, and more preferably 900 to 1000 W; the number of scans is preferably 45 to 55 times, and more preferably 50 to 55 times. In the present invention, when the barrier layer is a stacked NiV layer and an Al layer (i.e., NiV layer + Al layer), or a stacked NiV layer and a Cu layer (i.e., NiV layer + Cu layer), the sputtering power of the NiV layer is preferably 800-1200W, more preferably 900-1000W; the number of scans is preferably 25-35 times, more preferably 25-30 times; the sputtering power of the Al layer is preferably 1500-2000W, more preferably 1500-1700W; the number of scans is preferably 30-40 times, more preferably 30-35 times; the sputtering power of the Cu layer is preferably 1000-1600W, more preferably 1100-1200W; the number of scans is preferably 30-40 times, more preferably 30-35 times. In the present invention, the sputtering power of the Au layer is preferably 300-600W, more preferably 350-400W; the number of scans is preferably 180-220 times, more preferably 180-200 times. In the present invention, the sputtering power of the second TiW layer is preferably 800-1200W, more preferably 900-1000W; the number of scans is preferably 20-30 times, more preferably 23-26 times. In the present invention, the sputtering power of the Pt layer is preferably 600-1000W, more preferably 600-700W; the number of scans is preferably 80-100 times, more preferably 80-85 times. After the sputtering of the Pt layer is completed, the present invention preferably uses an X-ray thickness gauge to test the thickness of each layer, and the metallized ceramic substrate whose thickness meets the preset requirements is subjected to subsequent cutting processing steps.
[0038] After obtaining the metallized ceramic substrate, the present invention performs a slicing process on the metallized ceramic substrate to obtain the single-layer chip ceramic capacitor. The present invention preferably bonds the back side (i.e., the Pt layer) of the metallized ceramic substrate to the UV film, and performs the slicing process after the front side is reinforced with a transparent curing agent, and then uses ethanol, acetone, and deionized water to clean the slicing product in turn, and uses 25μm, 38μm, and 50μm gold wire bonding tension and ball push inspection according to customer requirements. The qualified products are tested for electrical performance according to process requirements, and the parameters are set to use an automatic testing machine to perform 100% testing on the product electrical performance indicators. The products that pass the electrical performance test are tested according to the appearance standards, and the appearance of the products is 100% tested using an automatic appearance testing machine. The products that pass the appearance test are packaged according to customer requirements using a packaging machine to obtain the single-layer chip ceramic capacitor. The thickness of the Pt layer in the present invention is ≤600nm, and it is not easy to curl during the slicing process, which is conducive to improving the slicing process pass rate and further saving costs.
[0039] At present, the traditional single-layer chip ceramic capacitors with TiW+Ni+Au film layer structure on both the front and back sides usually need to use photolithography and etching (or patterning) processes to produce patterns and then perform scribing. That is, after sputtering the film layer structures to obtain the metallized ceramic substrate, photolithography and patterning processes are usually required, and then scribing is performed; and because the back side is an Au layer and it is relatively thick (such as at least 3μm), and Au has good ductility, if the scribing process is performed directly, it will cause very serious "curling"; in addition, the front and back sides of the traditional single-layer chip ceramic capacitors are both Au layers, and can only be distinguished by the size of the electrodes on both sides, and the labor cost of picking is high. The front and back sides of the single-layer chip ceramic capacitor described in the present invention adopt different film layer structures, and the front and back sides can be easily distinguished without special patterns on the surface, thereby reducing the time cost and labor cost of subsequent particle picking. Moreover, after sputtering of each film layer structure to obtain a metallized ceramic substrate, it can be directly cut without the need for photolithography and patterning processes. Eliminating two processes is conducive to further reducing costs.
[0040] The present invention provides the application of the single-layer chip ceramic capacitor described in the above technical solution or the single-layer chip ceramic capacitor prepared by the preparation method described in the above technical solution in the field of semiconductor integrated circuits, 5G communications or aerospace. In the present invention, the single-layer chip ceramic capacitor can be specifically used in optical modules, power amplifier modules or TR components in radar equipment.
[0041] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] Example 1
[0043] In this embodiment, the front side of the single-layer chip ceramic capacitor adopts a TiW+Cu+NiV+Au film structure, and the back side adopts a TiW+Pt film structure. Specifically, from the front side to the back side, the single-layer chip ceramic capacitor includes an Au layer, a NiV layer (the mass ratio of Ni to V is 93:7), a Cu layer, a first TiW layer (the mass ratio of Ti to W is 95:5), a ceramic substrate, a second TiW layer (the mass ratio of Ti to W is 95:5) and a Pt layer stacked in sequence; the preparation method of the single-layer chip ceramic capacitor is as follows:
[0044] (1) Place a 150 μm thick ceramic substrate in a quartz boat cleaning fixture, and then place it in the alkaline cleaning solution (mainly potassium hydroxide) tank in the cleaning machine, set the ultrasonic current to 2.0 A, and start shaking cleaning for 15 minutes. After the alkaline cleaning solution is cleaned, place it in a deionized water rinse tank for 5 minutes. Repeat the above cleaning process 4 times, then place it in a 70°C high-temperature deionized water tank, set the ultrasonic current to 1.8 A, and start shaking cleaning for 15 minutes. After the cleaning is completed, the ceramic substrate is blown dry with nitrogen and transmitted after passing the cleanliness inspection;
[0045] (2) placing the cleaned ceramic substrate in a quartz boat, and then placing it in a high-temperature baking furnace, heating it uniformly from room temperature to 800°C over 180 minutes, keeping it warm and baking it for 60 minutes, then cooling it down to room temperature with the furnace and taking it out;
[0046] (3) After baking, the ceramic substrate is placed on the sputtering machine tray, sent into the process chamber and evacuated. When the vacuum degree in the process chamber is lower than 7.0×10 -7Torr, and then argon (Ar) is introduced, and the coating is carried out by scanning sputtering. Specifically, the first TiW layer, Cu layer, NiV layer and Au layer are sputtered in sequence on the front side of the ceramic substrate, and then the second TiW layer and Pt layer are sputtered in sequence on the back side of the ceramic substrate to obtain a metallized ceramic substrate; wherein the sputtering power of the first TiW layer is 1000W, the process gas pressure is 7mTorr, and the number of scans is 23 to 26 times; the sputtering power of the Cu layer is 1200W, the process gas pressure is 5mTorr, and the number of scans is 30 to 35 times; the sputtering power of the NiV layer is 1000W, the process gas pressure is 5mTorr, and the number of scans is 25 to 30 times; the sputtering power of the Au layer is 400W, the process gas pressure is 5mTorr, and the number of scans is 25 to 30 times. The gas pressure is 5mTorr, and the number of scans is 180 to 200 times; the sputtering power of the second TiW layer is 1000W, the process gas pressure is 7mTorr, and the number of scans is 23 to 26 times; the sputtering power of the Pt layer is 600W, the process gas pressure is 5mTorr, and the number of scans is 80 to 85 times; after sputtering, the thickness of each layer in the metallized ceramic substrate is tested by an X-ray thickness gauge: the thickness of the first TiW layer is 100 to 150nm, the thickness of the Cu layer is 450 to 600nm, the thickness of the NiV layer is 400 to 500nm, the thickness of the Au layer is 1300 to 1500nm, the thickness of the second TiW layer is 100 to 150nm, and the thickness of the Pt layer is 300 to 400nm;
[0047] (4) The back side (i.e., the Pt layer) of the metallized ceramic substrate is bonded to a UV film (purchased from Dongguan Changfeng New Materials Co., Ltd., model HPV-2667), and the front side is reinforced with a transparent curing agent and then scribed. The scribed product is then cleaned with ethanol, acetone, and deionized water in sequence. According to customer requirements, 25 μm, 38 μm, and 50 μm gold wire bonding tension and ball push tests are used, and the qualified ones are transferred to the next level;
[0048] (5) Test the electrical performance of the products that have been cut and cleaned according to the process requirements, set the parameters and use the automatic testing machine to test the electrical performance indicators of the products 100%, and download them after they pass the test;
[0049] (6) The products that have passed the electrical performance test are tested 100% according to the appearance standards using an automatic appearance tester, and the qualified ones are downloaded;
[0050] (7) Products that pass the appearance test are packaged using a packaging machine according to customer requirements.
[0051] Example 2
[0052] The front side of the single-layer chip ceramic capacitor in this embodiment adopts a TiW+Al+NiV+Au film structure, and the back side adopts a TiW+Pt film structure. Specifically, from the front side to the back side, the single-layer chip ceramic capacitor includes an Au layer, a NiV layer (the mass ratio of Ni to V is 93:7), an Al layer, a first TiW layer (the mass ratio of Ti to W is 95:5), a ceramic substrate, a second TiW layer (the mass ratio of Ti to W is 95:5) and a Pt layer stacked in sequence;
[0053] The preparation method of the single-layer chip ceramic capacitor refers to Example 1, except that the sputtered Cu layer is replaced by a sputtered Al layer, the sputtering power of the Al layer is 1500W, the process gas pressure is 5mTorr, and the number of scans is 30 to 35 times; after sputtering, an X-ray thickness gauge is used to test the thickness of each layer in the metallized ceramic substrate: the thickness of the first TiW layer is 100 to 150nm, the thickness of the Al layer is 450 to 500nm, the thickness of the NiV layer is 400 to 500nm, the thickness of the Au layer is 1300 to 1500nm, the thickness of the second TiW layer is 100 to 150nm, and the thickness of the Pt layer is 300 to 400nm.
[0054] Example 3
[0055] The front side of the single-layer chip ceramic capacitor in this embodiment adopts a TiW+NiV+Au film structure, and the back side adopts a TiW+Pt film structure. Specifically, from the front side to the back side, the single-layer chip ceramic capacitor includes an Au layer, a NiV layer (the mass ratio of Ni to V is 93:7), a first TiW layer (the mass ratio of Ti to W is 95:5), a ceramic substrate, a second TiW layer (the mass ratio of Ti to W is 95:5) and a Pt layer stacked in sequence;
[0056] The preparation method of the single-layer chip ceramic capacitor refers to Example 1, except that the sputtering of the Cu layer is omitted; the sputtering power of the NiV layer is 1000W, the process gas pressure is 5mTorr, and the number of scans is 50 to 55 times; after sputtering, the thickness of each layer in the metallized ceramic substrate is tested using an X-ray thickness gauge: the thickness of the first TiW layer is 100 to 150nm, the thickness of the NiV layer is 950 to 1100nm, the thickness of the Au layer is 100 to 150nm nm, the thickness of the second TiW layer is 100 to 150nm, and the thickness of the Pt layer is 300 to 400nm.
[0057] Comparative Example 1
[0058] The front and back sides of the single-layer chip ceramic capacitor in this comparative example both adopt a TiW+Ni+Au film structure. Specifically, from the front side to the back side, the single-layer chip ceramic capacitor includes a first Au layer, a first Ni layer, a first TiW layer (the mass ratio of Ti to W is 10:90), a ceramic substrate, a second TiW layer (the mass ratio of Ti to W is 10:90), a second Ni layer and a second Au layer stacked in sequence; the preparation method of the single-layer chip ceramic capacitor is as follows:
[0059] (1) Cleaning the ceramic substrate according to the method of step (1) in Example 1;
[0060] (2) baking the ceramic substrate according to the method of step (2) in Example 1;
[0061] (3) After baking, the ceramic substrate is placed on the sputtering machine tray, sent into the process chamber and evacuated. When the vacuum degree in the process chamber is lower than 7.0×10 -7 Torr, argon (Ar) was introduced, and the coating was carried out by scanning sputtering. Specifically, the first TiW layer, the first Ni layer and the first Au layer were sputtered in sequence on the front side of the ceramic substrate, and then the second TiW layer, the second Ni layer and the second Au layer were sputtered in sequence on the back side of the ceramic substrate to obtain a metallized ceramic substrate; the sputtering power of the first TiW layer and the second TiW layer was 1000W, the process gas pressure was 7mTorr, and the number of scans was 23 to 26 times; the sputtering power of the first Ni layer and the second Ni layer was 800W. , the process gas pressure is 5mTorr, and the number of scans is 35 to 40 times; the sputtering power of the first Au layer and the second Au layer is 400W, the process gas pressure is 5mTorr, and the number of scans is 400 to 420 times; after sputtering, the thickness of each layer in the metallized ceramic substrate is tested using an X-ray thickness gauge: the thickness of the first TiW layer and the second TiW layer is 100 to 150nm, the thickness of the first Ni layer and the second Ni layer is 350 to 400nm, and the thickness of the first Au layer and the second Au layer is 3500 to 4000nm;
[0062] (4) The metallized ceramic substrate is placed in a deionized water rinse tank and rinsed for 5 minutes. After being blown dry with nitrogen, it is sent to a coater, and photoresist is evenly dropped on the center of the front side of the metallized ceramic substrate. The coater is rotated at 3500 rpm to coat. After the coating is completed, it is placed in an oven and dried at 150° C. for 2 minutes. Then, the back side of the metallized ceramic substrate is processed according to the above coating and drying operations. After that, the corresponding mask is assembled and exposed using a double-sided photolithography machine for 20 seconds. After the exposure is completed, it is placed in a developer for development for 75 seconds. After the development is completed, it is placed in a deionized water rinse tank and rinsed for 5 minutes. After being blown dry with nitrogen, it is placed in an oven and dried at 110° C. for 2 minutes to obtain a photolithography ceramic substrate;
[0063] (5) placing the photolithography ceramic substrate in an Au layer etching solution for etching for 120 to 130 seconds, placing it in a Ni layer etching solution for etching for 300 to 330 seconds, and placing it in a TiW layer etching solution for etching for 65 to 75 seconds, and then placing it in a degumming solution to remove excess photoresist on the pattern. After the degumming is completed, place it in a deionized water rinse tank for rinsing for 5 minutes, and blow dry it with nitrogen to obtain a patterned ceramic substrate (or etched ceramic substrate);
[0064] (6) The back side of the patterned ceramic substrate is bonded to a UV film (purchased from Dongguan Changfeng New Materials Co., Ltd., model number HPV-2667), and the front side is reinforced with a transparent curing agent and then scribed. The scribed product is then cleaned with ethanol, acetone, and deionized water in sequence. According to customer requirements, 25 μm, 38 μm, and 50 μm gold wire bonding tension and ball push tests are used, and the qualified ones are transferred to the next level;
[0065] (7) Test the electrical performance of the products that have been cut and cleaned according to the process requirements, set the parameters and use an automatic testing machine to test the electrical performance indicators of the products 100%, and download them after they pass the test;
[0066] (8) The products that have passed the electrical performance test are tested 100% according to the appearance standards using an automatic appearance tester, and the qualified ones are downloaded;
[0067] (9) Products that pass the appearance test are packaged using a packaging machine according to customer requirements.
[0068] The performance test results of the products prepared in Examples 1 to 3 and Comparative Example 1 are shown in Table 1, wherein each test item is tested in accordance with GJB2442A-2021; at least 100 products are taken for testing in each Example and Comparative Example. As can be seen from Table 1, the electrical performance indicators, solderability, and reliability verification of the single-layer chip ceramic capacitor provided by the present invention are consistent with those of the front and back TiW+Ni+Au film structure products.
[0069] Table 1 Performance test results of products prepared in Examples 1 to 3 and Comparative Example 1
[0070]
[0071]
[0072] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A single-layer chip ceramic capacitor, characterized in that: It comprises an Au layer, a barrier layer, a first TiW layer, a ceramic substrate, a second TiW layer and a Pt layer which are stacked in sequence, wherein the barrier layer comprises a NiV layer, the thickness of the Au layer is ≤2000nm, and the thickness of the Pt layer is ≤600nm.
2. The single-layer chip ceramic capacitor according to claim 1, characterized in that: The barrier layer further includes an Al layer or a Cu layer stacked with the NiV layer. When the barrier layer includes the Al layer or the Cu layer, the NiV layer is in contact with the Au layer.
3. The single-layer chip ceramic capacitor according to claim 2, characterized in that: The thickness of the barrier layer is 500-1500 nm; the thickness of the Al layer and the Cu layer are independently 200-600 nm.
4. The single-layer chip ceramic capacitor according to any one of claims 1 to 3, characterized in that: The NiV layer is formed of a NiV alloy, and the mass fraction of Ni in the NiV alloy is 90-95%.
5. The single-layer chip ceramic capacitor according to claim 1 or 2, characterized in that: The first TiW layer and the second TiW layer are formed of a TiW alloy, and the mass fraction of Ti in the TiW alloy forming the first TiW layer and the second TiW layer is independently 80-95%.
6. The single-layer chip ceramic capacitor according to claim 5, characterized in that: The thickness of the first TiW layer and the second TiW layer are independently 50-200 nm.
7. The single-layer chip ceramic capacitor according to claim 1, 2, 3 or 6, characterized in that: The thickness of the Au layer is 1300-2000 nm, and the thickness of the Pt layer is 300-600 nm.
8. The method for preparing the single-layer chip ceramic capacitor according to any one of claims 1 to 7, characterized in that: The following steps are involved: sputtering a first TiW layer, a barrier layer, and an Au layer in sequence on one surface of a ceramic substrate, and sputtering a second TiW layer and a Pt layer in sequence on the other surface of the ceramic substrate to obtain a metallized ceramic substrate; The metallized ceramic substrate is subjected to a dicing process to obtain the single-layer chip ceramic capacitor.
9. The preparation method according to claim 8, characterized in that: The sputtering method of the first TiW layer, the barrier layer, the Au layer, the second TiW layer and the Pt layer is a scanning sputtering method; The sputtering power of the first TiW layer is 800-1200W, and the number of scans is 20-30 times; The sputtering power of the Au layer is 300-600W, and the number of scans is 180-220 times; The sputtering power of the second TiW layer is 800-1200W, and the number of scans is 20-30 times; The sputtering power of the Pt layer is 600-1000W, and the number of scans is 80-100 times; When the barrier layer is a NiV layer, the sputtering power of the barrier layer is 800 to 1200 W, and the number of scans is 45 to 55 times; When the barrier layer is a stacked NiV layer and an Al layer, or a stacked NiV layer and a Cu layer, the sputtering power of the NiV layer is 800-1200W, and the scanning number is 25-35 times; the sputtering power of the Al layer is 1500-2000W, and the scanning number is 30-40 times; the sputtering power of the Cu layer is 1000-1600W, and the scanning number is 30-40 times.
10. Application of the single-layer chip ceramic capacitor according to any one of claims 1 to 7 or the single-layer chip ceramic capacitor prepared by the preparation method according to claim 8 or 9 in semiconductor integrated circuits, 5G communications or aerospace fields.